MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Radici Radilon® Aestus T1 RV400RKC 306 BK Polyphthalamide
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 40% Glass Fiber Reinforced

Material Notes: PPA injection molding grade 40% glass fiber reinforced with high glass transition temperature and high melting point. Black color.

Suitable for parts requiring high stiffness and strength. High resistance to hot water contact, suitable for drinking water contact.

Information provided by Radici Group.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.52 g/ccDAM; ISO 1183
Water Absorption 0.10 %
@Thickness 2.00 mm,
Time 86400 sec
Immersion @ 23°C; ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.0070 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 225 MPa5mm / min. Conditioned; ISO 527-2/1A
 230 MPa5mm / min. DAM; ISO 527-2/1A
Elongation at Break 2.0 %5 mm / min. Conditioned; ISO 527-2/1A
 2.1 %5 mm / min. DAM; ISO 527-2/1A
Tensile Modulus 14750 MPa1mm / min. Conditioned; ISO 527-2/1A
 14800 MPa1mm / min. DAM; ISO 527-2/1A
Flexural Strength 310 MPa2mm / min. DAM; ISO 178
Flexural Modulus 12800 MPa2mm / min. DAM; ISO 178
Charpy Impact Unnotched 55.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eU
 65.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 9.50 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1e/A
 10.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1e/A
 11.0 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1e/A
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmDAM; 500V.; IEC 60093
Surface Resistance 1.00e+12 ohmDAM; 500V.; IEC 60093
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 17.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
CTE, linear, Transverse to Flow 58.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
Melting Point 325 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 293 °CISO 75/2Af
Flammability, UL94 HB
@Thickness 0.800 mm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 330 - 350 °CInjection Molding
Mold Temperature 140 - 160 °C
 
Descriptive Properties
Injection Molding Injection SpeedHigh

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PRADI6936 / 293441

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.