MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Adaptive3D Soft ToughRubber™ Elastomer for DLP
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Adaptive 3D® Soft ToughRubber™ is an innovative polymer resin that enables customers to produce flexible end parts and products at scale with high accuracy, isotropic properties, and great printability. This elastomer ensures the silicone feel and mechanical properties of the DLP® printing's resolution and surface finish even when manufacturing complex geometry parts or models. Soft ToughRubber is the newest product in the ToughRubber family. It is a class of one-part, one-pot, rapid curing photopolymers with high-throughput print speeds. Designed for functional prototypes of audio ear buds, wearable electronics, and anatomical medical models Soft ToughRubber (STR) delivers silicone feel and mechanical properties with the resolution and surface finish that DLP® printing provides.

Applications: medical, transportation, consumer product, wearable electronics.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.019 g/ccLiquid; ASTM D792
Viscosity 560 cPLiquid as Supplied; ASTM D2196
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 24
@Time 10.0 sec
ASTM D2240
 36
@Time 0.000 sec
ASTM D2240
Tensile Strength, Ultimate 1.40 MPa
 1.40 MPaASTM D412 Method A Die C
 1.50 MPaASTM D638 Type V
Elongation at Break 255 %Method A Die C; ASTM D412
Tensile Modulus 0.800 MPaStorage; ASTM D4065
Resilience 4.0% Bayshore; ASTM D2632
 4.00[%], Bayshore; ASTM D2632
Tear Strength 5.00 kN/mDie C; ASTM D625
Compression Set 5.00 %
@Treatment Temp. 25.0 °C,
Time 79200 sec
ASTM D395 Method B Type 1
 10.0 %
@Treatment Temp. 70.0 °C,
Time 79200 sec
ASTM D395 Method B Type 1
 
Thermal PropertiesOriginal ValueComments
Glass Transition Temp, Tg -4.00 °CASTM D4065
 
Descriptive Properties
ColorBlack
Fracture Toughness1.6 MJ/m3ASTM D638 Type V
 1.7 MJ/m3ASTM D412 Method A Die C
Fracture Toughness (MJ/m3)1.7ASTM D638. Type V

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PADAPT90 / 305367

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.