MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
Ensinger TECAMID 66 GF35 black Nylon 66, 35% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Glass Fiber Filled

Material Notes:
  • very high stiffness
  • resistant to many oils, greases and fuels
  • good wear properties
  • very high strength
  • high dimensional stability
  • good heat deflection temperature
  • good weldable and bondable
Target Industries:
  • aircraft and aerospace technology
  • mechanical engineering

Information provided by Ensinger Inc.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.40 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 98.0 MPa50mm/min; DIN EN ISO 527-2
Elongation at Break 11 %50mm/min; DIN EN ISO 527-2
Elongation at Yield 7.0 %50mm/min; DIN EN ISO 527-2
Modulus of Elasticity 5.70 GPa1mm/min; DIN EN ISO 527-2
Flexural Strength 149 MPaDIN EN ISO 178
Flexural Modulus 5100 MPaDIN EN ISO 178
Charpy Impact Unnotched 80.0 kJ/m²DIN EN ISO 179-1eU
Charpy Impact, Notched 5.00 kJ/m²DIN EN ISO 179-1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+14 ohm-cmSilver electrode, 23°C, 12% r.h.; DIN IEC 60093
Surface Resistance 1.00e+14 ohmSilver electrode, 23°C, 12% r.h.; DIN IEC 60093
 
Thermal PropertiesOriginal ValueComments
Melting Point 254 °CDIN EN ISO 11357
Maximum Service Temperature, Air 110 °Clong term
 170 °Cshort term
Glass Transition Temp, Tg 48.0 °CDIN EN ISO 11357
Flammability, UL94 HBDIN IEC 60695-11-10
 
Descriptive Properties
Colorblack opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PENSIN8165 / 319093

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.