MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Pressure Seal 23625 Ethylene Propylene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 23625 is a 60 durometer white colored EPDM formulated with FDA sanctioned materials. This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 AA 610 A13 EA14 F17; 3 AA 610 B13 B33 EA14 F17; 2 BA 610 F17; 8 BA 610 B13

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.23 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 58
 59
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 64
@Temperature 70.0 °C,
Time 252000 sec
Heat Aged
 65
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 80
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 80
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 81
@Temperature 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 81
@Temperature 150 °C,
Time 252000 sec
Heat Aged
Tensile Strength 1037 psi
 1053.6 psi
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 1113.7 psi
@Temperature 70.0 °C,
Time 252000 sec
Heat Aged
 1186.3 psi
@Temperature 150 °C,
Time 252000 sec
Heat Aged
 1186.3 psi
@Temperature 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 1273.4 psi
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 1316 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 1316 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Elongation, Ultimate 450 %
 153.9 %
@Temperature 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 153.9 %
@Temperature 150 °C,
Time 252000 sec
Heat Aged
 260 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 260 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 419.8 %
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 450 %
@Temperature 70.0 °C,
Time 252000 sec
Heat Aged
 490.1 %
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
100% Modulus 247 psi
Tear Strength 78.0 pliDie B
Compression Set 16.5 %
@Temperature 70.0 °C,
Time 79200 sec
Solid
 17.2 %
@Temperature 100 °C,
Time 79200 sec
Solid
 18.7 %
@Temperature 70.0 °C,
Time 79200 sec
Plied
 21.4 %
@Temperature 100 °C,
Time 79200 sec
Plied
 30.6 %
@Temperature 100 °C,
Time 252000 sec
Plied
 34.3 %
@Temperature 125 °C,
Time 79200 sec
Plied
 49 %
@Temperature 150 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -71.0 °F
Shrinkage 2.0 %
@Temperature 100 °C,
Time 252000 sec
Volume, Distilled water aged
 
Descriptive Properties
ColorWhite

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL224 / 318434

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.