MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) AvaSpire® AV-848 Polyaryletherketone (PAEK), Unfilled
Categories: Polymer; Thermoplastic; Polyketone; Polyaryletherketone (PAEK), Unreinforced

Material Notes: AvaSpire® AV-848 is a high-temperature, polyaryletherketone (PAEK) that offers several key performance advantages over comparable grades of PEEK above 150°C, including better dimensional stability, lower CLTE from 150°C to 240°C, and lower modulus for greater flexibility at room temperature.

- Natural: AvaSpire® AV-848 NT

Markets/Uses: Oil & Gas / Down Hole / Back-Up Seal Rings

Applications: Oil/Gas Applications; Seals

Features: Chemical Resistant; Ductile; Fatigue Resistant; Flame Retardant; Good Dimensional Stability; Good Impact Resistance; High Heat Resistance

Injection notes: Back Pressure: Minimum

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.32 g/ccASTM D792
Water Absorption 0.50 %
@Time 86400 sec
ASTM D570
Viscosity 500 cPMelt; ASTM D3835
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 94.0 MPa50 mm/min; ASTM D638
Elongation at Break 75 %ASTM D638
Elongation at Yield 6.7 %50 mm/min; ASTM D638
Tensile Modulus 3100 MPa50 mm/min; ASTM D638
Flexural Strength 134 MPaASTM D790
Flexural Modulus 3300 MPaASTM D790
Compressive Strength 118 MPaASTM D695
Shear Strength 82.0 MPaASTM D732
Izod Impact, Notched 75.0 J/mASTM D256
Izod Impact, Unnotched NBASTM D256
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.18
@Frequency 1e+6 Hz
ASTM D150
 3.21
@Frequency 60 Hz
ASTM D150
 3.23
@Frequency 1000 Hz
ASTM D150
Dielectric Strength 180 kV/mm
@Thickness 0.0500 mm
Amorphous Film; ASTM D149
Dissipation Factor 0.0010
@Frequency 1000 Hz
ASTM D150
 0.0020
@Frequency 60 Hz
ASTM D150
 0.0060
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
Specific Heat Capacity 1.65 J/g-°C
@Temperature 50.0 °C
ASTM C351
 1.66 J/g-°C
@Temperature 200 °C
ASTM C351
Thermal Conductivity 0.220 W/m-KASTM C177
Melting Point 340 °CPeak; ASTM D3418
Deflection Temperature at 1.8 MPa (264 psi) 252 °CAnnealed; ASTM D648
Glass Transition Temp, Tg 158 °CDSC
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 366 °C
Middle Barrel Temperature 371 °C
Front Barrel Temperature 377 °C
Nozzle Temperature 382 °C
Melt Temperature 382 - 404 °CInjection
Mold Temperature 166 - 193 °C
Drying Temperature 149 °C
@Time 14400 sec
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorNatural Color
FormsPellets
Injection RateFast
ProcessingExtrusion Blow Molding; Fiber (Spinning) Extrusion; Film Extrusion; Injection Blow Molding
 Injection Molding; Machining; Profile Extrusion; Thermoforming; Wire & Cable Extrusion
Screw Compression Ratio2.0:1.0 to 3.0:1.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4160 / 279960

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.