MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

(Viewing data as-entered. Click here to return)
SABIC LNP™ THERMOCOMP™ GF006 PSU (Europe)  (Unverified Data**)
Categories: Polymer; Thermoplastic; Polysulfone (PSU); Polysulfone, 30% Glass Fiber Reinforced

Material Notes: LNP THERMOCOMP* GF006 is a compound based on Polysulfone resin containing 30% Glass Fiber.

Information provided by SABIC

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.47 g/ccISO 1183
 1.49 g/ccISO 1183
Water Absorption 0.26 %
@Time 86400 sec
ISO 62-1
Linear Mold Shrinkage, Flow 0.0010 - 0.0040 cm/cmSABIC method
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 118 MPa5 mm/min; ISO 527
Elongation at Break 1.6 %5 mm/min; ISO 527
Flexural Yield Strength 165 MPa2 mm/min; ISO 178
Flexural Modulus 8900 MPa2 mm/min; ISO 178
Flexural Strain at Break 2.2 %2 mm/min; ISO 178
Izod Impact, Notched (ISO) 8.00 kJ/m²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 29.0 kJ/m²80*10*4; ISO 180/1U
 30.0 kJ/m²80*10*4; ISO 180/1U
Tangent Modulus 10000 MPa1 mm/min; ISO 527
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 20.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 59.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 184 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
Deflection Temperature at 1.8 MPa (264 psi) 182 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
Flammability, UL94 V-0
@Thickness 1.60 mm
UL 94 by SABIC-IP
 
Processing PropertiesOriginal ValueComments
Zone 1 325 - 340 °C
Zone 2 340 - 350 °C
Zone 3 350 - 360 °C
Melt Temperature 360 - 370 °C
Mold Temperature 150 °C
Drying Temperature 120 - 150 °C
Dry Time 4.00 hour
Moisture Content 0.050 %
Back Pressure 0.200 - 0.300 MPa
Screw Speed 30 - 60 rpm

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
LNP Thermocomp® GF-1006 Polysulfone, Glass Fiber Reinforcement
Syensqo (Solvay Specialty Polymers) Mindel® B-322 Polysulfone, Modified (PSU, Modified)
RTP Company RTP 2000 B-430 Polysulfone Alloy Glass Fiber - Flame Retardant

PSABI21204 / 214340

Ensinger SPI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.