MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Pressure Seal 23844 Ethylene Propylene
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 23844 is an 80 durometer black colored EPDM elastomer, it is formulated with FDA sanctioned materials. It exhibits excellent resistance to heat, compression set and boiling water. It will remain non brittle at very low temperatures. This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 AA 815 A13 F17 EA14; 2 BA 815 F17; 4 BA 815 A14 F17; 7 BA 815; 6 CA 810 A25 B35 F17 G11 G21 EA14; 7 CA 815 A25 B35 F17 F18 G11 G21 EA14; 8 CA 815 A25 B35 F17 G11 G21; 2 DA 815 A26 B36 F19 G11 G21 EA14; 3 DA 815 A26 B36 F19 G11 G21 EA14

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.16 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 82
 82
@Temperature 70.0 °C,
Time 252000 sec
Heat Aged
 82
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 83
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 83
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 83
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 85
@Temperature 150 °C,
Time 252000 sec
Heat Aged
 85
@Temperature 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
Tensile Strength 1998 psi
 1628.4 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 1628.4 psi
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 1940 psi
@Temperature 70.0 °C,
Time 252000 sec
Heat Aged
 1968 psi
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 2061.9 psi
@Temperature 150 °C,
Time 252000 sec
Heat Aged
 2061.9 psi
@Temperature 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 2289.7 psi
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
Elongation, Ultimate 192 %
 167 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 167 %
@Temperature 125 °C,
Time 252000 sec
Heat Aged
 187 %
@Temperature 100 °C,
Time 252000 sec
Heat Aged
 188 %
@Temperature 150 °C,
Time 252000 sec
Heat Aged
 188 %
@Temperature 150 °C,
Time 252000 sec
Heat Aged, Test Tube Method
 191.04 %
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 192 %
@Temperature 70.0 °C,
Time 252000 sec
Heat Aged
100% Modulus 839 psi
Tear Strength 149 pliDie B
 165 pliDie C
Compression Set 7.2 %
@Temperature 100 °C,
Time 79200 sec
Solid
 7.8 %
@Temperature 70.0 °C,
Time 79200 sec
Solid
 9.8 %
@Temperature 125 °C,
Time 79200 sec
Solid
 9.8 %
@Temperature 100 °C,
Time 252000 sec
Solid
 12.3 %
@Temperature 100 °C,
Time 79200 sec
Plied
 13.4 %
@Temperature 70.0 °C,
Time 79200 sec
Plied
 13.6 %
@Temperature 125 °C,
Time 79200 sec
Plied
 21.9 %
@Temperature 150 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature <= -76.0 °F
Shrinkage -0.300 %
@Temperature 100 °C,
Time 252000 sec
Volume, Distilled water aged
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL235 / 318445

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.