MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Greene Tweed CHEMRAZ® 510 Perfluoroelastomer
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: Greene Tweed’s Chemraz® 510, a perfluoroelastomer, offers an extremely broad range of chemical resistance with a Shore A hardness value of 90. with a temperature range form -22°F to 446°F (-30°C to 230°C), Chemraz 510 is well suited for use in a range of applications, from mechanical seals to pump housings.

Because of its versatility, Chemraz 510 is often used as a standard compound for sealing at high pressures. It can be found in a variety of fluids and solutions including acids, caustics, aldehydes, esters, aromatics, hot water, steam, amines, methanol, ketones, TBA and many other custom shapes.

Applications:

  • Mechanical seals
  • Valves
  • Pump Housings
  • Sampling/metering equipment
  • Compressors
  • Reactors
  • Mixers
  • Controls/instrumentation
  • Sprayers/dispensers
  • Couplings

Information provided by Greene Tweed.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.92 g/cc1.92 g/ccASTM D297
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9090ASTM D2240
Tensile Strength at Break 13.62 MPa1975 psiASTM D1414
Tensile Strength, Yield 7.58 MPa1100 psi@ 50% Elongation; ASTM D1414
Elongation at Break 85 %85 %ASTM D1414
Compression Set 30 %
@Temperature 204 °C,
Time 252000 sec
30 %
@Temperature 400 °F,
Time 70.0 hour
At 25% deflection; ASTM D395
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 230 °C446 °F
Minimum Service Temperature, Air -30.0 °C-22.0 °F
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Greene Tweed CHEMRAZ® 526 Perfluoroelastomer
Greene Tweed CHEMRAZ® 615 Perfluoroelastomer
Eagle Brass 316L Austenitic Stainless Steel, 1/8 Hardened
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Condition H 1150 (Heated 621°C)
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Condition H 1150M (Heated 760°C/2hr/AC then 621°C/4hr/AC)

PGREEN02 / 42296

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.