MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Ascend Performance Materials HiDura™ MED AP NT0860 PA66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Unreinforced

Material Notes: HiDura MED AP NT0860 is an unfilled resin designed for healthcare applications. It is a lubricated PA66 resin with fast cycle times even in large cavitation tools for higher productivity and can easily be colored. This product offers a combination of engineering properties characterized by high strength; rigidity; good toughness; high melt point; good surface lubricity; abrasion resistance; and resistance to many chemicals including disinfectants. The product is compliant to ISO 10993-5 and ISO 10993-10. It exhibits good property retention after most sterilization methods.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.14 g/ccDAM; ISO 1183
Water Absorption 1.2 %
@Time 86400 sec
DAM; ISO 62
Moisture Absorption at Equilibrium 2.4 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.020 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.020 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 49.0 MPa50% RH; ISO 527-2
 81.0 MPaDAM; ISO 527-2
Tensile Strength, Yield 60.0 MPa50% RH; ISO 527-2
 89.0 MPaDAM; ISO 527-2
Elongation at Break 29 %DAM; ISO 527-2
 76 %50% RH; ISO 527-2
Elongation at Yield 4.8 %DAM; ISO 527-2
 20 %50% RH; ISO 527-2
Tensile Modulus 1900 MPa50% RH; ISO 527-2
 2900 MPaDAM; ISO 527-2
Flexural Strength 30.0 MPa50% RH; ISO 178
 105 MPaDAM; ISO 178
Flexural Modulus 1100 MPa50% RH; ISO 178
 3300 MPaDAM; ISO 178
Poissons Ratio 0.40ISO 527-2
Izod Impact, Notched (ISO) 5.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 6.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 7.00 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 180/1A
 23.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Charpy Impact Unnotched NB
@Temperature -30.0 °C
50% RH; ISO 179/1eU
 NB
@Temperature -30.0 °C
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
50% RH; ISO 179/1eU
 NB
@Temperature 23.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 5.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 6.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 7.00 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 23.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 100 µm/m-°C
@Thickness 2.00 mm,
Temperature 35.0 - 55.0 °C
DAM; ISO 11359-2
CTE, linear, Transverse to Flow 100 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
DAM; ISO 11359-2
Melting Point 260 °CDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 210 °CUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 72.0 °CUnannealed; DAM; ISO 75-2/A
Oxygen Index 26 %Railway Application; DAM; EN ISO 4589-2
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 260 - 280 °CInjection
Middle Barrel Temperature 270 - 285 °CInjection
Front Barrel Temperature 280 - 290 °CInjection
Nozzle Temperature 280 - 300 °CInjection
Melt Temperature 285 - 300 °CInjection
Mold Temperature 65.0 - 95.0 °CInjection
Drying Temperature 70.0 °CInjection
Dry Time 1.00 - 3.00 hourInjection
 
Descriptive Properties
AdditiveLubricant
 Release agent
Agency RatingsBSE/TSE Compliant
 ISO, 1043 PA66
AppearanceNatural Color
FeaturesAbrasion Resistance
 Balanced Stiffness/Toughness
 Bromine Free
 Chemical Resistant
 Corrosion Resistant
 Ductile
 Excellent Processability
 Fast Molding Cycle
 Good Colorability
 Good Electrical Properties
 Good Flow
 Good Mold Release
 Good Rigidity
 Good Stiffness
 Good Surface Finish
 Halogen Content, None
 High Crystallinity
 High Toughness
 Homopolymer
 Ignition Resistant
 Lubricated
 Medium Viscosity
 Nucleated
 Solvent Resistant
FormsPellets
Processing MethodInjection Molding
 Profile Extrusion
RegionNorth America, Europe, Asia Pacific
 South and Central America, Near East/Africa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PASCE8505 / 296297

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.