MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
SABIC NORYL™ Resin FP5140 Polyphenylene Ether + PS (PPE+PS) (Europe)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene + Polyphenylene Ether, Unreinforced

Material Notes: NORYL™ FP5140 resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This injection moldable grade contains non-brominated, non-chlorinated flame retardant with a UL94 flame rating of V1 at 1.5mm NORYL FP5140 resin was designed to have very good dimensional stability with high flow and exhibits good rheological properties, high heat resistance, hydrolysis resistance, and very low density. The combination of these properties makes this material an excellent candidate for Flat Panel TV enclosure applications.

Features: Hydrolytic Stability,Low Creep Sensitivity,Flame Retardant,Non-Halogenated,Non-Chlorinated,Non-Brominated,Low Warpage,High Flow,Good Processability

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.11 g/ccASTM D792
Density 1.11 g/ccISO 1183
Moisture Absorption 0.0500 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.18 %ISO 62-1
Viscosity 15 cP
@Load 1.20 kg,
Temperature 280 °C
MVR cc/10 min; ISO 1133
 44 cP
@Load 2.16 kg,
Temperature 280 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
SABIC method
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 48.0 MPa50 mm/min; ISO 527
Tensile Strength, Yield 58.0 MPa50 mm/min; ISO 527
Elongation at Break 7.0 %50 mm/min; ISO 527
Elongation at Yield 3.5 %50 mm/min; ISO 527
Tensile Modulus 2450 MPa1 mm/min; ISO 527
 2940 MPa50 mm/min; ASTM D638
Flexural Strength 87.0 MPayield, 2 mm/min; ISO 178
Flexural Modulus 2300 MPa2 mm/min; ISO 178
Izod Impact, Notched (ISO) 6.00 kJ/m²80*10*4; ISO 180/1A
 4.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Charpy Impact, Notched 5.00 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 3.00e+16 - 3.50e+16 ohm-cmASTM D257
 3.00e+16 - 3.50e+16 ohm-cmIEC 60093
Surface Resistance 8.00e+13 - 8.50e+13 ohmASTM D257
 8.00e+16 - 8.50e+16 ohmROA; IEC 60093
Dielectric Constant 2.8
@Frequency 1e+6 Hz
IEC 60250
 3.0
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 27.5 kV/mm
@Thickness 1.60 mm
in oil; IEC 60243-1
Dissipation Factor 0.0020
@Frequency 1e+6 Hz
ASTM D150
 0.0020
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 250 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 83.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 83.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 77.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 77.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 81.0 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 103 °CRate B/50; ASTM D1525
 105 °CRate B/50; ISO 306
 110 °CRate B/120; ISO 306
UL RTI, Electrical 65.0 °CUL 746B
UL RTI, Mechanical with Impact 65.0 °CUL 746B
UL RTI, Mechanical without Impact 65.0 °CUL 746B
Flammability, UL94 V-2
@Thickness >=1.00 mm
UL 94
 V-1
@Thickness >=1.50 mm
UL 94
 V-0
@Thickness >=2.00 mm
UL 94
Oxygen Index 30 %ISO 4589
Glow Wire Ignition Temperature 700 °C
@Thickness 1.00 mm
IEC 60695-2-13
 725 °C
@Thickness 2.00 mm
IEC 60695-2-13
 725 °C
@Thickness 3.00 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 3.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 240 - 270 °C
Zone 2 230 - 260 °C
Zone 3 250 - 285 °C
Melt Temperature 250 - 285 °CInjection Molding
Mold Temperature 40.0 - 65.0 °C
Drying Temperature 70.0 - 80.0 °CInjection Molding
Dry Time 2.00 - 3.00 hourInjection Molding
Precipitation Temperature 60.0 - 80.0 °CHopper Temperature

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH82302 / 290249

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.