MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

USP Class VI Adhesives
USP Class VI Approved Adhesives for Medical Device Applications
Master Bond’s biocompatible adhesives are designed to meet the needs of medical device manufacturers. Compounds withstand various types of sterilization methods.

(Viewing data as-entered. Click here to return)
SABIC GELOY CR7500 ASA (Asia Pacific)  (Unverified Data**)
Categories: Polymer; Thermoplastic; ASA Polymer

Material Notes: High heat ASA with optimum flow-impact balance. For Automotive applications and Automotive colors only.

Information provided by SABIC Innovative Plastics for Asia Pacific.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.08 g/ccASTM D 792
Density 1.07 g/ccISO 1183
Moisture Absorption 0.200 %
@Temperature 23.0 °C
50% RH; ISO 62
Water Absorption at Saturation 0.50 %
@Temperature 23.0 °C
ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC Method
Melt Flow 6.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
cm^3/10 min Melt Volume Rate; ISO 1133
 6.3 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ASTM D 1238
 10 g/10 min
@Load 5.00 kg,
Temperature 260 °C
cm^3/10 min Melt Volume Rate; ISO 1133
 11 g/10 min
@Load 5.00 kg,
Temperature 260 °C
ASTM D 1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 33.0 MPaType I, 5 mm/min; ASTM D 638
 35.0 MPa5 mm/min; ISO 527
Tensile Strength, Yield 40.0 MPaType I, 5 mm/min; ASTM D 638
 43.0 MPa5 mm/min; ISO 527
Elongation at Break 19 %5 mm/min; ISO 527
 60 %Type I, 5 mm/min; ASTM D 638
Elongation at Yield 3.3 %5 mm/min; ISO 527
 3.6 %Type I, 5 mm/min; ASTM D 638
Tensile Modulus 1970 MPa5 mm/min; ASTM D 638
 2040 MPa1 mm/min; ISO 527
Flexural Yield Strength 64.0 MPa2 mm/min; ISO 178
 68.0 MPa1.3 mm/min, 50 mm span; ASTM D 790
Flexural Modulus 2060 MPa2 mm/min; ISO 178
 2170 MPa1.3 mm/min, 50 mm span; ASTM D 790
Izod Impact, Notched 60.0 J/m
@Temperature -30.0 °C
ASTM D 256
 400 J/m
@Temperature 23.0 °C
ASTM D 256
Izod Impact, Notched (ISO) 6.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
 15.0 kJ/m²
@Temperature 23.0 °C
80*10*4; ISO 180/1A
Charpy Impact, Notched 14.0 kJ/m²
@Temperature 23.0 °C
V-notch Edgew 80*10*4 sp=62mm; ISO 179/1eA
Instrumented Impact Total Energy 30.0 J
@Temperature 23.0 °C
ASTM D 3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 84.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E 831
 84.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 95.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E 831
 95.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
Hot Ball Pressure Test <= 98.0 °CIEC 60695-10-2
Deflection Temperature at 1.8 MPa (264 psi) 88.0 °CEdgew 120*10*4 sp=100mm; ISO 75/Ae
 89.0 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 90.0 °C
@Thickness 3.20 mm
unannealed; ASTM D 648
Vicat Softening Point 98.0 °CRate B/50; ASTM D 1525
 102 °CRate B/50; ISO 306
 105 °CRate B/120; ISO 306

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chi Mei Kibilac® PW-978D ASA, High Heat
Chi Mei Kibilac® PW-978B ASA, High Heat
Trinseo EMERGE™ 5302 Acrylonitrile Butadiene Styrene (ABS)
LG Chemical PT270 ABS
LG Chemical LI921NS ASA

PSABI47655 / 188740

USP Class VI adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.