System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Radici Radilon® A 42K 100 M NT Polyamide 66
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 66 (PA66)
;
Nylon 66, Extruded
;
Nylon 66, Heat Stabilized
Material Notes:
PA66 high viscosity extrusion grade. Heat stabilized. Natural color. Suitable for extrusion of tubes, profiles, bars, rods and sheets. Also suitable for injection molding of high thickness items.
Information provided by Radici Group.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
1.14
g/cc
DAM; ISO 1183
Water Absorption
8.4 %
@Thickness 2.00 mm,
Temperature 23.0 °C
Immersion; ISO 62
Moisture Absorption
2.10 %
@Thickness 2.00 mm,
Temperature 23.0 °C
50% RH; ISO 62
Viscosity Test
260
cm³/g
Viscosity Index; Sulfuric Acid; ISO 307
Linear Mold Shrinkage, Flow
0.011
cm/cm
DAM; ISO 294-4
0.013
cm/cm
Conditioned; ISO 294-4
Linear Mold Shrinkage, Transverse
0.013
cm/cm
ISO 294-4
Mechanical Properties
Original Value
Comments
Tensile Strength, Yield
60.0
MPa
50mm/min. Conditioned; ISO 527-2/1A
85.0
MPa
50mm/min. DAM; ISO 527-2/1A
Elongation at Break
45 %
50mm / min. DAM; ISO 527-2/1A
>= 50 %
50 mm / min. Conditioned; ISO 527-2/1A
Elongation at Yield
4.5 %
DAM; ISO 527-2/1A
25 %
Conditioned; ISO 527-2/1A
Tensile Modulus
1600
MPa
1mm / min. Conditioned; ISO 527-2/1A
3200
MPa
1mm / min. DAM; ISO 527-2/1A
Flexural Strength
110
MPa
2mm / min. DAM; ISO 178
Flexural Modulus
2900
MPa
2mm / min. DAM; ISO 178
Charpy Impact, Notched
5.00
kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1e/A
6.00
kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1e/A
20.0
kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1e/A
Electrical Properties
Original Value
Comments
Volume Resistivity
1.00e+11
ohm-cm
Conditioned. 500V; IEC 60093
1.00e+13
ohm-cm
DAM; 500V.; IEC 60093
Surface Resistance
1.00e+10
ohm
Conditioned; IEC 60093
1.00e+12
ohm
DAM; 500V.; IEC 60093
Thermal Properties
Original Value
Comments
Melting Point
260
°C
10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi)
195
°C
ISO 75/2Bf
Deflection Temperature at 1.8 MPa (264 psi)
75.0
°C
ISO 75/2Af
Vicat Softening Point
240
°C
@Load 5.10 kg
50°C/h; ISO 306
Flammability, UL94
HB
@Thickness 0.800 mm
Flame Spread
0.000
mm/min
@Thickness 3.00 mm
Automotive Interior; ISO 3795
Glow Wire Flammability Index
750
°C
@Thickness 2.00 mm
IEC 60695-2-1/2
Processing Properties
Original Value
Comments
Processing Temperature
270
-
290
°C
Extrusion Temperature
Melt Temperature
280
-
300
°C
Injection Molding
Mold Temperature
70.0
-
90.0
°C
Descriptive Properties
Injection Molding Injection Speed
Medium
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
PRADI6911 / 293416
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.