System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
SABIC LNP™ LUBRICOMP™ Compound PDXF89080 Polyethylene, Unspecified (PE, Unspecified)
Categories:
Polymer
;
Thermoplastic
;
Polyethylene (PE)
Material Notes:
LNP LUBRICOMP PDXF89080 compound is based on Polyethylene (PE) resin containing proprietary fillers. Added features of this grade include: Wear Resistant.
Features: Wear resistant
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
0.920
g/cc
0.920
g/cc
ASTM D792
Density
0.920
g/cc
0.0332
lb/in³
ASTM D792
Moisture Absorption
0.0300 %
0.0300 %
23°C/50% RH/24 hrs; ASTM D570
0.0300 %
0.0300 %
23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow
0.020
-
0.040
cm/cm
0.020
-
0.040
in/in
24hrs; ASTM D955
Linear Mold Shrinkage, Transverse
0.010
-
0.030
cm/cm
0.010
-
0.030
in/in
24hrs; ASTM D955
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
8.00
MPa
1160
psi
5 mm/min; ISO 527
9.00
MPa
1310
psi
5 mm/min; ASTM D638
Tensile Strength, Yield
9.00
MPa
1310
psi
5 mm/min; ISO 527
10.0
MPa
1450
psi
5 mm/min; ASTM D638
Elongation at Break
90 %
90 %
5 mm/min; ASTM D638
164 %
164 %
5 mm/min; ISO 527
Elongation at Yield
73 %
73 %
5 mm/min; ASTM D638
88 %
88 %
5 mm/min; ISO 527
Tensile Modulus
0.200
GPa
29.0
ksi
5 mm/min; ASTM D638
0.240
GPa
34.8
ksi
1 mm/min; ISO 527
Flexural Strength
5.00
MPa
725
psi
ISO 178
Flexural Modulus
0.120
GPa
17.4
ksi
1.3 mm/min, 50 mm span; ASTM D790
0.120
GPa
17.4
ksi
2 mm/min; ISO 178
Izod Impact Notched
304
J
224
ft-lb
ASTM D256
Izod Impact, Unnotched
NB
NB
ASTM D4812
Izod Impact, Notched (ISO)
37.0
kJ/m²
17.6
ft-lb/in²
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO)
NB
NB
80*10*4; ISO 180/1U
Dart Drop, Total Energy
19.0
J
14.0
ft-lb
ASTM D3763
Impact Test
19.0
J
14.0
ft-lb
Multiaxial Impact; ISO 6603
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
208
µm/m-°C
@Temperature -30.0 - 30.0 °C
116
µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
CTE, linear, Transverse to Flow
199
µm/m-°C
@Temperature -30.0 - 30.0 °C
111
µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi)
41.0
°C
106
°F
Flatw 80*10*4 sp=64mm; ISO 75/Bf
42.0
°C
@Thickness 3.20 mm
108
°F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
23.0
°C
73.4
°F
Flatw 80*10*4 sp=64mm; ISO 75/Af
23.0
°C
@Thickness 3.20 mm
73.4
°F
@Thickness 0.126 in
unannealed; ASTM D648
Processing Properties
Metric
English
Comments
Zone 2
210
-
220
°C
410
-
428
°F
Zone 3
220
-
230
°C
428
-
446
°F
Melt Temperature
230
°C
446
°F
Injection Molding
Mold Temperature
40.0
-
55.0
°C
104
-
131
°F
Drying Temperature
80.0
°C
176
°F
Injection Molding
Dry Time
4.00
hour
4.00
hour
Injection Molding
Back Pressure
0.200
-
0.300
MPa
29.0
-
43.5
psi
Screw Speed
30
-
60
rpm
30
-
60
rpm
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABH80935 / 288882
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.