MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Syensqo (Solvay Specialty Polymers) Ryton® XK2340 PPS Alloy, 40% glass filled, high strength
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS)

Material Notes: 40% glass filled PPS alloy with high strength, exceptionally high flow and precision molding; black color

Ryton® XK2340 40% glass fiber reinforced polyphenylene sulfide alloy compound provides excellent mechanical strength, toughness, and rigidity, along with excellent flow in thin-walled parts, low flash characteristics, and fast cycle times. It may be easily molded in conventional injection molding equipment utilizing water heated molds.

Markets/Uses: Automotive / Automotive E/E / Engine Control Units

Applications: Automotive Applications

Features: Fast Molding Cycle; Good Flow; Good Strength; Good Toughness; High Rigidity

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.56 g/ccASTM D792
Water Absorption 0.30 %
@Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.0030 cm/cm
@Thickness 3.20 mm
ASTM D955
Linear Mold Shrinkage, Transverse 0.0060 cm/cm
@Thickness 3.20 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 95ASTM D785
Hardness, Rockwell R 115ASTM D785
Tensile Strength 193 MPaASTM D638
Tensile Stress 195 MPaISO 527-2
Elongation at Break 1.8 %ASTM D638
 1.8 %ISO 527-2
Flexural Strength 255 MPaASTM D790
 270 MPaISO 178
Flexural Modulus 12000 MPaISO 178
 12400 MPaASTM D790
Compressive Strength 255 MPaASTM D695
Poissons Ratio 0.42ASTM E132
Izod Impact, Notched 85.0 J/m
@Thickness 3.18 mm
ASTM D256
Izod Impact, Unnotched 640 J/m
@Thickness 3.18 mm
ASTM D256
Izod Impact, Notched (ISO) 8.50 kJ/m²Notch A; ISO 180
Izod Impact, Unnotched (ISO) 35.0 kJ/m²ISO 180
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+14 ohm-cmASTM D257
Surface Resistance 1.00e+15 ohmASTM D257
Insulation Resistance 1.00e+12 ohm
@Temperature 90.0 °C
IEC 60167
Dielectric Constant 3.9
@Frequency 1e+6 Hz
ASTM D150
 4.3
@Frequency 1000 Hz
ASTM D150
Dielectric Strength 22.0 kV/mmASTM D149
Dissipation Factor 0.010
@Frequency 1e+6 Hz
ASTM D150
 0.020
@Frequency 1000 Hz
ASTM D150
Arc Resistance 100 secASTM D495
Comparative Tracking Index 275 VUL 746
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 15.0 µm/m-°C
@Temperature 100 - 200 °C
ASTM E831
 20.0 µm/m-°C
@Temperature -50.0 - 50.0 °C
ASTM E831
CTE, linear, Transverse to Flow 55.0 µm/m-°C
@Temperature -50.0 - 50.0 °C
ASTM E831
 100 µm/m-°C
@Temperature 100 - 200 °C
ASTM E831
Thermal Conductivity 0.340 W/m-KASTM C177
Deflection Temperature at 1.8 MPa (264 psi) 245 °CUnannealed; ASTM D648
Flammability, UL94 HB
@Thickness 1.60 mm
Oxygen Index 35 %ASTM D2863
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorBlack
FormsPellets
ProcessingInjection Molding
RoHS ComplianceYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSOL8Y4463 / 280263

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.