Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.19 g/cc | 1.19 g/cc |
Density | 1.20 g/cc | 0.0434 lb/in³ |
Moisture Absorption | 0.0200 % | 0.0200 % |
| 0.110 % | 0.110 % |
Water Absorption at Saturation | 0.14 % | 0.14 % |
Viscosity | 29 cP @Load 1.20 kg, Temperature 300 °C | 29 cP @Load 2.65 lb, Temperature 572 °F |
Linear Mold Shrinkage, Flow | 0.0055 - 0.0075 cm/cm @Thickness 3.20 mm | 0.0055 - 0.0075 in/in @Thickness 0.126 in |
Linear Mold Shrinkage, Transverse | 0.0060 - 0.0080 cm/cm @Thickness 3.20 mm | 0.0060 - 0.0080 in/in @Thickness 0.126 in |
Melt Flow | 30 g/10 min @Load 1.20 kg, Temperature 300 °C | 30 g/10 min @Load 2.65 lb, Temperature 572 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Tensile Strength at Break | 51.0 MPa | 7400 psi |
| 56.0 MPa | 8120 psi |
Tensile Strength, Yield | 63.0 MPa | 9140 psi |
| 66.0 MPa | 9570 psi |
Elongation at Break | 55 % | 55 % |
| 78 % | 78 % |
Elongation at Yield | 6.0 % | 6.0 % |
| 6.0 % | 6.0 % |
Tensile Modulus | 2.20 GPa | 319 ksi |
| 2.45 GPa | 355 ksi |
Flexural Strength | 97.0 MPa | 14100 psi |
| 105 MPa | 15200 psi |
Flexural Modulus | 2.37 GPa | 344 ksi |
| 2.40 GPa | 348 ksi |
Izod Impact Notched | 100 J | 73.8 ft-lb |
| 90.0 J @Temperature -30.0 °C | 66.4 ft-lb @Temperature -22.0 °F |
Izod Impact, Unnotched | NB | NB |
| NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
Izod Impact, Notched (ISO) | 10.0 kJ/m² | 4.76 ft-lb/in² |
| 10.0 kJ/m² @Temperature -30.0 °C | 4.76 ft-lb/in² @Temperature -22.0 °F |
Izod Impact, Unnotched (ISO) | NB | NB |
| NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
Charpy Impact Unnotched | NB | NB |
| NB @Temperature -30.0 °C | NB @Temperature -22.0 °F |
Charpy Impact, Notched | 3.00 J/cm² | 14.3 ft-lb/in² |
| 1.00 J/cm² @Temperature -30.0 °C | 4.76 ft-lb/in² @Temperature -22.0 °F |
Dart Drop, Total Energy | 60.0 J | 44.3 ft-lb |
|
Electrical Properties | Metric | English | Comments |
---|
Dielectric Constant | 2.78 @Frequency 1.10e+9 Hz | 2.78 @Frequency 1.10e+9 Hz |
Dissipation Factor | 0.0056 @Frequency 1.10e+9 Hz | 0.0056 @Frequency 1.10e+9 Hz |
Comparative Tracking Index | 175 - 250 V | 175 - 250 V |
Hot Wire Ignition, HWI | 15 - 30 sec @Thickness >=0.400 mm | 15 - 30 sec @Thickness >=0.0157 in |
| 30 - 60 sec @Thickness >=1.70 mm | 30 - 60 sec @Thickness >=0.0669 in |
High Amp Arc Ignition, HAI | 30 - 60 arcs @Thickness >=0.400 mm | 30 - 60 arcs @Thickness >=0.0157 in |
| 60 - 120 arcs @Thickness >=2.00 mm | 60 - 120 arcs @Thickness >=0.0787 in |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 68.0 µm/m-°C @Temperature -40.0 - 40.0 °C | 37.8 µin/in-°F @Temperature -40.0 - 104 °F |
| 78.0 µm/m-°C @Temperature 23.0 - 80.0 °C | 43.3 µin/in-°F @Temperature 73.4 - 176 °F |
CTE, linear, Transverse to Flow | 70.0 µm/m-°C @Temperature -40.0 - 40.0 °C | 38.9 µin/in-°F @Temperature -40.0 - 104 °F |
| 76.0 µm/m-°C @Temperature 23.0 - 80.0 °C | 42.2 µin/in-°F @Temperature 73.4 - 176 °F |
Hot Ball Pressure Test | 125 °C | 257 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 130 °C | 266 °F |
| 130 °C @Thickness 3.20 mm | 266 °F @Thickness 0.126 in |
Deflection Temperature at 1.8 MPa (264 psi) | 120 °C | 248 °F |
| 120 °C @Thickness 3.20 mm | 248 °F @Thickness 0.126 in |
Vicat Softening Point | 136 °C | 277 °F |
| 138 °C | 280 °F |
| 140 °C | 284 °F |
UL RTI, Electrical | 130 °C | 266 °F |
UL RTI, Mechanical with Impact | 120 °C | 248 °F |
UL RTI, Mechanical without Impact | 130 °C | 266 °F |
Flammability, UL94 | V-2 @Thickness >=0.400 mm | V-2 @Thickness >=0.0157 in |
| V-1 @Thickness >=1.70 mm | V-1 @Thickness >=0.0669 in |
| V-0 @Thickness >=2.00 mm | V-0 @Thickness >=0.0787 in |
Glow Wire Ignition Temperature | 850 °C @Thickness 1.70 mm | 1560 °F @Thickness 0.0669 in |
| 850 °C @Thickness 2.00 mm | 1560 °F @Thickness 0.0787 in |
| 850 °C @Thickness 3.00 mm | 1560 °F @Thickness 0.118 in |
Glow Wire Flammability Index | 960 °C @Thickness 1.70 mm | 1760 °F @Thickness 0.0669 in |
| 960 °C @Thickness 2.00 mm | 1760 °F @Thickness 0.0787 in |
| 960 °C @Thickness 3.00 mm | 1760 °F @Thickness 0.118 in |
|
Optical Properties | Metric | English | Comments |
---|
Transmission, Visible | >= 88 % @Thickness 3.00 mm | >= 88 % @Thickness 0.118 in |
| >= 89 % @Thickness 2.00 mm | >= 89 % @Thickness 0.0787 in |
| >= 90 % @Thickness 1.00 mm | >= 90 % @Thickness 0.0394 in |
|
Processing Properties | Metric | English | Comments |
---|
Nozzle Temperature | 275 - 300 °C | 527 - 572 °F |
Zone 2 | 270 - 295 °C | 518 - 563 °F |
Zone 3 | 280 - 305 °C | 536 - 581 °F |
Melt Temperature | 280 - 305 °C | 536 - 581 °F |
Mold Temperature | 70.0 - 95.0 °C | 158 - 203 °F |
Drying Temperature | 120 °C | 248 °F |
Dry Time | 3.00 - 4.00 hour | 3.00 - 4.00 hour |
| 48.0 hour | 48.0 hour |
Back Pressure | 0.300 - 0.700 MPa | 43.5 - 102 psi |
Shot Size | 40 - 60 % | 40 - 60 % |
Vent Depth | 0.00250 - 0.00760 cm | 0.000984 - 0.00299 in |
Screw Speed | 40 - 70 rpm | 40 - 70 rpm |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.