SABIC LNP™ LUBRICOMP™ Compound NXCY620 Polycarbonate + ABS (PC+ABS)
Categories:
Polymer
;
Thermoplastic
;
ABS Polymer
;
Polycarbonate/ABS Alloy, Unreinforced
Material Notes:
LNP LUBRICOMP NXCY620 compound is based on Polycarbonate/Acrylonitrile Butadiene Styrene (PC/ABS) blend containing silicone. Added features of this grade include: Wear Resistant.
Features: Wear resistant
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.14
g/cc
1.14
g/cc
ASTM D792
Density
1.13
g/cc
0.0408
lb/in³
ASTM D792
Moisture Absorption
0.0200 %
0.0200 %
Injection Molding
0.150 %
0.150 %
23°C/50% RH/24 hrs; ASTM D570
Linear Mold Shrinkage, Flow
0.0060
-
0.0080
cm/cm
0.0060
-
0.0080
in/in
24hrs; ASTM D955
Linear Mold Shrinkage, Transverse
0.0060
-
0.0080
cm/cm
0.0060
-
0.0080
in/in
24hrs; ASTM D955
Melt Flow
30
g/10 min
@Load 5.00 kg,
Temperature 260 °C
30
g/10 min
@Load 11.0 lb,
Temperature 500 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
40.0
MPa
5800
psi
5 mm/min; ASTM D638
42.0
MPa
6090
psi
5 mm/min; ISO 527
Tensile Strength, Yield
49.0
MPa
7110
psi
5 mm/min; ISO 527
51.0
MPa
7400
psi
5 mm/min; ASTM D638
Elongation at Break
31 %
31 %
50 mm/min; ASTM D638
50 %
50 %
50 mm/min; ISO 527
Elongation at Yield
4.7 %
4.7 %
50 mm/min; ASTM D638
4.9 %
4.9 %
50 mm/min; ISO 527
Tensile Modulus
2.09
GPa
303
ksi
1 mm/min; ISO 527
2.19
GPa
318
ksi
5 mm/min; ASTM D638
Flexural Strength
77.0
MPa
11200
psi
ISO 178
79.0
MPa
11500
psi
brk, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus
2.11
GPa
306
ksi
2 mm/min; ISO 178
2.22
GPa
322
ksi
1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched
654
J
482
ft-lb
ASTM D256
Izod Impact, Unnotched
NB
NB
ASTM D4812
Izod Impact, Notched (ISO)
48.0
kJ/m²
22.8
ft-lb/in²
80*10*4; ISO 180/1A
28.0
kJ/m²
@Temperature -40.0 °C
13.3
ft-lb/in²
@Temperature -40.0 °F
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO)
NB
NB
80*10*4; ISO 180/1U
Charpy Impact, Notched
5.10
J/cm²
24.3
ft-lb/in²
ISO 179/2C
3.90
J/cm²
@Temperature -30.0 °C
18.6
ft-lb/in²
@Temperature -22.0 °F
ISO 179/2C
Coefficient of Friction, Dynamic
0.23
0.23
ASTM D3702 Modified: Manual
Coefficient of Friction, Static
0.18
0.18
ASTM D3702 Modified: Manual
K (wear) Factor
14.1
x 10
-8
mm³/N-M
7.00
x 10
-10
in³-min/ft-lb-hr
Ring; ASTM D3702 Modified: Manual
2520
x 10
-8
mm³/N-M
1250
x 10
-10
in³-min/ft-lb-hr
Washer; ASTM D3702 Modified: Manual
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
73.0
µm/m-°C
@Temperature -30.0 - 30.0 °C
40.6
µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
CTE, linear, Transverse to Flow
78.0
µm/m-°C
@Temperature -30.0 - 30.0 °C
43.3
µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi)
125
°C
257
°F
Flatw 80*10*4 sp=64mm; ISO 75/Bf
Deflection Temperature at 1.8 MPa (264 psi)
110
°C
230
°F
Flatw 80*10*4 sp=64mm; ISO 75/Af
108
°C
@Thickness 3.20 mm
226
°F
@Thickness 0.126 in
unannealed; ASTM D648
Processing Properties
Metric
English
Comments
Nozzle Temperature
240
-
280
°C
464
-
536
°F
Zone 2
250
-
290
°C
482
-
554
°F
Zone 3
250
-
290
°C
482
-
554
°F
Melt Temperature
260
-
290
°C
500
-
554
°F
Injection Molding
Mold Temperature
60.0
-
90.0
°C
140
-
194
°F
Drying Temperature
95.0
-
105
°C
203
-
221
°F
Injection Molding
Dry Time
2.00
-
4.00
hour
2.00
-
4.00
hour
Injection Molding
Precipitation Temperature
60.0
-
80.0
°C
140
-
176
°F
Hopper Temperature
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABH80908 / 288855
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.