MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Zotefoams Plastazote® MP15FR Metallocene Polyethylene Foam, Flame Retardant
Categories: Polymer; Thermoplastic; Polyethylene (PE); Low Density (LDPE)

Material Notes: Plastazote® is a closed cell, cross-linked polyethylene foam manufactured using nitrogen expansion technology to produce foams with exceptional cell size uniformity, low odor / high purity and outstanding physical attributes.

Compliant with EC food contact regulations.

Information provided by Zotefoams

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.0150 g/cc0.000542 lb/in³Nominal skin/skin; BS ISO 7214 1998
 0.0140 - 0.0180 g/cc0.000506 - 0.000650 lb/in³sheet density
Cell Length 0.200 - 0.600 mm0.00787 - 0.0236 in
 0.900 mm0.0354 inTypical Diameter
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore OO 262610 mm cell/cell thickness; ISO 868 1985
Tensile Strength 0.353 MPa51.2 psiISO 7214 1998
Elongation at Break 146 %146 %
Compressive Yield Strength  0.0180 MPa
@Strain 10 %
2.61 psi
@Strain 10 %
BS ISO 7214 1998
 0.0350 MPa
@Strain 25 %
5.08 psi
@Strain 25 %
BS ISO 7214 1998
 0.0620 MPa
@Strain 40 %
8.99 psi
@Strain 40 %
BS ISO 7214 1998
 0.0890 MPa
@Strain 50 %
12.9 psi
@Strain 50 %
BS ISO 7214 1998
Tear Strength 0.545 kN/m3.11 pliBS EN ISO 8067 1995
Compression Set  5.0 %
@Time 79200 sec,
Strain 25 %
5.0 %
@Time 22.0 hour,
Strain 25 %
24 hr recovery; BS ISO 7214 1998
 18 %
@Time 79200 sec,
Strain 25 %
18 %
@Time 22.0 hour,
Strain 25 %
0.5 hr recovery; BS ISO 7214 1998
 26.5 %
@Time 79200 sec,
Strain 50 %
26.5 %
@Time 22.0 hour,
Strain 50 %
24 hr recovery; BS ISO 7214 1998
 38 %
@Time 79200 sec,
Strain 50 %
38 %
@Time 22.0 hour,
Strain 50 %
0.5 hr recovery; BS ISO 7214 1998
 
Thermal PropertiesMetricEnglishComments
Thermal Conductivity 0.0390 W/m-K0.271 BTU-in/hr-ft²-°Fmean temp of 10°C; ISO 8302 1991
Maximum Service Temperature, Air 95.0 °C203 °F
Minimum Service Temperature, Air -70.0 °C-94.0 °F
Flammability Test  2.6
@Thickness 13.0 mm
2.6
@Thickness 0.512 in
Horizontal Burn Rate, mm/sec; ISO 7214 1998
 4.0
@Thickness 5.00 mm
4.0
@Thickness 0.197 in
Horizontal Burn Rate, mm/sec; ISO 7214 1998
 
Descriptive Properties
FlammabilityAutomotive: FMVSS.302 burn ratePass: > 3 mm thick
 Aviation: CAA8/2-2.2bComplies
 Construction: DIN4102 B1Pass: 6 to 20 mm thick

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Makrolon® 6870 Polycarbonate
Zotefoams Plastazote® HL34 Polyethylene Foam
Zotefoams Plastazote® LD33 Low Density Polyethylene Foam
Zotefoams Plastazote® LD18 Low Density Polyethylene Foam
Zotefoams Plastazote® HL79 Polyethylene Foam

PZOTEF937 / 150693

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.