MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LEXAN™ FR Resin FXD153 Polycarbonate (PC) (Americas)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: FXD153 is an Extrusion / Blow molding grade in a Diffusion effect, which is part of the VisualFX family. These effects have been developed to meet increasing Aesthetic demands in the Marketplace. Color Package may affect properties, Application testing always reccomended.

Features: Aesthetics & Visual effects

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.0200 %0.0200 %Extrusion Blow Molding
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 2.5 g/10 min
@Load 1.20 kg,
Temperature 300 °C
2.5 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 66.0 MPa9570 psi50 mm/min; ASTM D638
Tensile Strength, Yield 62.0 MPa8990 psi50 mm/min; ASTM D638
Elongation at Break 110 %110 %50 mm/min; ASTM D638
Elongation at Yield 7.0 %7.0 %50 mm/min; ASTM D638
Tensile Modulus 2.34 GPa339 ksi5 mm/min; ASTM D638
Flexural Strength 93.0 MPa13500 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.34 GPa339 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 748 J552 ft-lbASTM D256
Izod Impact, Unnotched 32.04 J/cm60.02 ft-lb/inASTM D4812
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Transverse to Flow 68.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
37.8 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 138 °C
@Thickness 3.20 mm
280 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 132 °C
@Thickness 3.20 mm
270 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 157 °C315 °FRate B/50; ASTM D1525
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 315 - 340 °C599 - 644 °F
Zone 1 260 - 290 °C500 - 554 °FExtrusion Blow Molding
Zone 2 260 - 290 °C500 - 554 °FExtrusion Blow Molding
 310 - 330 °C590 - 626 °F
Zone 3 260 - 290 °C500 - 554 °FExtrusion Blow Molding
 320 - 345 °C608 - 653 °F
Zone 4 260 - 290 °C500 - 554 °FExtrusion Blow Molding
Zone 5 260 - 290 °C500 - 554 °F
Melt Temperature 265 - 280 °C509 - 536 °FExtrusion Blow Molding
 320 - 345 °C608 - 653 °FInjection Molding
Mold Temperature 60.0 - 100 °C140 - 212 °F
 80.0 - 115 °C176 - 239 °F
Drying Temperature 120 °C248 °FInjection Molding
 120 °C248 °FExtrusion Blow Molding
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourExtrusion Blow Molding
 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 48.0 hour48.0 hourCumulative; Injection Molding
Moisture Content 0.010 %0.010 %minimum
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 40 - 60 %40 - 60 %
Vent Depth 0.00250 - 0.00760 cm0.000984 - 0.00299 in
Screw Speed 40 - 70 rpm40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80485 / 288432

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.