MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Ascend Performance Materials ReDefyne™ IAG25 BK0806 PA66-I-GF25
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Glass Reinforced, Impact Grade

Material Notes: IAG25 BK0806 - ReDefyne is a (PA66 + PA6)-GF25 glass fiber filled black industrial recycled grade with added impact for flexibility and strength

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.31 g/ccDAM; ISO 1183
Water Absorption 1.2 %
@Time 86400 sec
DAM; ISO 62
Moisture Absorption at Equilibrium 1.7 %DAM to 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0090 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.012 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 89.0 MPa50% RH; ISO 527-2
 135 MPaDAM; ISO 527-2
Elongation at Break 3.1 %DAM; ISO 527-2
 6.9 %50% RH; ISO 527-2
Tensile Modulus 5500 MPa50% RH; ISO 527-2
 8000 MPaDAM; ISO 527-2
Flexural Strength 113 MPa50% RH; ISO 178
 190 MPaDAM; ISO 178
Flexural Modulus 4900 MPa50% RH; ISO 178
 7000 MPaDAM; ISO 178
Izod Impact, Notched (ISO) 5.90 kJ/m²
@Temperature -40.0 °C
DAM; ISO 180/1A
 6.50 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 7.10 kJ/m²
@Temperature -40.0 °C
50% RH; ISO 180/1A
 7.80 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 180/1A
 12.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 14.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Charpy Impact Unnotched 58.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eU
 60.0 kJ/m²
@Temperature -40.0 °C
50% RH; ISO 179/1eU
 61.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eU
 63.0 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eU
 78.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
 85.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eU
Charpy Impact, Notched 6.80 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 7.10 kJ/m²
@Temperature -40.0 °C
50% RH; ISO 179/1eA
 7.20 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eA
 8.50 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 13.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 17.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 21.0 kV/mm
@Thickness 1.00 mm
50% RH; IEC 60243
 38.0 kV/mm
@Thickness 1.00 mm
DAM; IEC 60243
 
Thermal PropertiesOriginal ValueComments
Melting Point 262 °CDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 254 °CUnannealed; 50% RH; ISO 75-2/B
 254 °CUnannealed; DAM; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 233 °CUnannealed; 50% RH; ISO 75-2/A
 238 °CUnannealed; DAM; ISO 75-2/A
 
Descriptive Properties
AdditiveLubricant
AppearanceBlack
FeaturesBalanced Stiffness/Toughness
 Bromine Free
 General Purpose
 Good Color Stability
 Good Dimensional Stability
 Good Impact Strength
 Good Mold Release
 Good Processability
 Good Rigidity
 Good Stiffness
 Good Strength
 Good Surface Finish
 Good Tensile Strength
 Good Toughness
 Halogen Content, None
 Lubricated
 Medium Viscosity
 Non-Corrosive
FormsPellets
Processing MethodInjection Molding
 Profile Extrusion
RegionNorth America, Europe, Asia Pacific

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PASCE9050 / 287550

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.