MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
SABIC Cycoloy® CY6120 PC+ABS  (Unverified Data**)
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced; Polycarbonate (PC)

Material Notes: Non-chlorinated and non-brominated flame retardant PC/ABS featuring good flow and impact properties. UL-94 V0 listed at 1.2mm intended for various thin wall applications.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.19 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0030 - 0.0050 cm/cm
@Thickness 3.20 mm
SABIC Method
Melt Flow 18 g/10 min
@Load 2.16 kg,
Temperature 260 °C
ASTM D1238
Melt Index of Compound 16 g/10 min
@Load 2.16 kg,
Temperature 260 °C
MVR [cm^3/10 min]; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 49.0 MPa50 mm/min; ISO 527
 59.0 MPaType I, 50 mm/min; ASTM D638
Tensile Strength, Yield 58.0 MPa50 mm/min; ISO 527
 62.0 MPaType I, 50 mm/min; ASTM D638
Elongation at Break 100 %Type I, 50 mm/min; ASTM D638
 100 %50 mm/min; ISO 527
Elongation at Yield 4.0 %Type I, 50 mm/min; ASTM D638
 4.0 %50 mm/min; ISO 527
Tensile Modulus 2600 MPa1 mm/min; ISO 527
 2960 MPa50 mm/min; ASTM D638
Flexural Yield Strength 93.0 MPa2 mm/min; ISO 178
 102 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2500 MPa2 mm/min; ISO 178
 2820 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 587 J/mASTM D256
Izod Impact, Notched (ISO) 40.0 kJ/m²80*10*4; ISO 180/1A
Dart Drop, Total Energy 54.0 J
@Temperature 23.0 °C
ASTM D3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant 2.6
@Frequency 1e+6 Hz
IEC 60250
 2.7
@Frequency 50.0 - 60.0 Hz
IEC 60250
Dielectric Strength 17.0 kV/mm
@Thickness 3.20 mm
in oil; IEC 60243-1
Dissipation Factor 0.0041
@Frequency 50.0 - 60.0 Hz
IEC 60250
 0.0086
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 73.8 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E 831
 80.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 80.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 84.6 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E 831
Deflection Temperature at 0.46 MPa (66 psi) 93.0 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 85.0 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 95.0 °CRate B/50; ISO 306
 96.0 °CRate B/50; ASTM D1525
 98.0 °CRate B/120; ISO 306
UL RTI, Electrical 60.0 °CUL 746B
UL RTI, Mechanical with Impact 60.0 °CUL 746B
UL RTI, Mechanical without Impact 60.0 °CUL 746B
Flammability, UL94 V-0
@Thickness 1.19 mm
UL 94

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Covestro Bayblend® FR 3008 Polycarbonate + ABS, Flame Retardant Grade

PSABI51087 / 151133

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.