SABIC LNP™ LUBRICOMP™ Compound PFL36 Polyamide 6 (Nylon 6) (Asia)
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 6 (PA6)
Material Notes:
LNP LUBRICOMP PFL36 compound is based on Nylon 6 resin containing 30% glass fiber, 15% PTFE. Added features of this grade include: Wear Resistant.
Features: Wear resistant,Structural
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Moisture Absorption
0.150 - 0.250 %
0.150 - 0.250 %
Injection Molding
Linear Mold Shrinkage, Flow
0.0010
cm/cm
0.0010
in/in
SABIC method
Linear Mold Shrinkage, Transverse
0.0070
cm/cm
0.0070
in/in
SABIC method
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
150
MPa
21800
psi
5 mm/min; ASTM D638
155
MPa
22500
psi
5 mm/min; ISO 527
Tensile Strength, Yield
150
MPa
21800
psi
5 mm/min; ASTM D638
155
MPa
22500
psi
5 mm/min; ISO 527
Elongation at Break
3.2 %
3.2 %
5 mm/min; ISO 527
3.3 %
3.3 %
5 mm/min; ASTM D638
Elongation at Yield
2.9 %
2.9 %
5 mm/min; ASTM D638
2.9 %
2.9 %
5 mm/min; ISO 527
Tensile Modulus
10.1
GPa
1460
ksi
5 mm/min; ASTM D638
10.2
GPa
1480
ksi
1 mm/min; ISO 527
Flexural Strength
210
MPa
30500
psi
brk, 1.3 mm/min, 50 mm span; ASTM D790
215
MPa
31200
psi
yld, 1.3 mm/min, 50 mm span; ASTM D790
235
MPa
34100
psi
break, 2mm/min; ISO 178
235
MPa
34100
psi
yield, 2 mm/min; ISO 178
Flexural Modulus
7.50
GPa
1090
ksi
1.3 mm/min, 50 mm span; ASTM D790
8.60
GPa
1250
ksi
2 mm/min; ISO 178
Izod Impact Notched
95.0
J
70.1
ft-lb
ASTM D256
Izod Impact, Unnotched
10.0
J/cm
18.7
ft-lb/in
ASTM D4812
Izod Impact, Notched (ISO)
12.0
kJ/m²
5.71
ft-lb/in²
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO)
75.0
kJ/m²
35.7
ft-lb/in²
80*10*4; ISO 180/1U
Charpy Impact Unnotched
7.50
J/cm²
35.7
ft-lb/in²
Edgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched
1.10
J/cm²
5.23
ft-lb/in²
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Coefficient of Friction, Dynamic
0.67
0.67
ASTM D3702 Modified: Manual
Coefficient of Friction, Static
0.87
0.87
ASTM D3702 Modified: Manual
K (wear) Factor
36.3
x 10
-8
mm³/N-M
18.0
x 10
-10
in³-min/ft-lb-hr
Washer; ASTM D3702 Modified: Manual
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
24.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
13.3
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
24.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
13.3
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow
96.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
53.3
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
96.0
µm/m-°C
@Temperature -40.0 - 40.0 °C
53.3
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi)
215
°C
419
°F
Flatw 80*10*4 sp=64mm; ISO 75/Bf
215
°C
@Thickness 3.20 mm
419
°F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
200
°C
392
°F
Flatw 80*10*4 sp=64mm; ISO 75/Af
205
°C
@Thickness 3.20 mm
401
°F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point
210
°C
410
°F
Rate B/50; ASTM D1525
210
°C
410
°F
Rate B/50; ISO 306
Processing Properties
Metric
English
Comments
Zone 2
265
-
275
°C
509
-
527
°F
Zone 3
275
-
290
°C
527
-
554
°F
Melt Temperature
265
-
275
°C
509
-
527
°F
Injection Molding
Mold Temperature
80.0
-
95.0
°C
176
-
203
°F
Drying Temperature
80.0
°C
176
°F
Injection Molding
Dry Time
4.00
hour
4.00
hour
Injection Molding
Back Pressure
0.300
-
0.700
MPa
43.5
-
102
psi
Screw Speed
30
-
60
rpm
30
-
60
rpm
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABH80939 / 288886
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.