MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
BASF Ultramid® B3WG7 Nylon 6, 35% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 40% Glass Fiber Filled

Material Notes: Ultramid B3WG7 is a 35% glass fiber reinforced injection molding PA6 grade for highly rigid, dimensionally stable components which are resistant to high temperature aging and have improved retention of properties in a hot water environment.

Applications: Typical applications include automotive clutch and accelerator pedals

Information provided by BASF.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.41 g/ccISO 1183
Moisture Absorption 2.00 %50% RH; ISO 62
Water Absorption at Saturation 6.2 %ISO 62
Melt Flow 45 g/10 min
@Load 5.00 kg,
Temperature 275 °C
Dry; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 130 MPaConditioned; ISO 527
 195 MPaDry; ISO 527
Elongation at Break 3.5 %
@Temperature 23.0 °C
Dry; ISO 527
 3.8 %
@Temperature -40.0 °C
Dry; ISO 527
 7.0 %
@Temperature 23.0 °C
Conditioned; ISO 527
Tensile Modulus 7200 MPaConditioned; ISO 527
 11000 MPaDry; ISO 527
Flexural Modulus 10000 MPaDry; ISO 178
Charpy Impact Unnotched 90.0 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179
 100 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179
 110 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179
Charpy Impact, Notched 13.0 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179
 18.0 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179
 33.0 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+10 ohm-cmConditioned; IEC 60093
 1.00e+13 ohm-cmDry; IEC 60093
Dielectric Constant 3.9
@Frequency 1e+6 Hz
Dry; IEC 60250
 6.2
@Frequency 1e+6 Hz
Conditioned; IEC 60250
Dissipation Factor 0.021
@Frequency 100 Hz
Dry; IEC 60250
 0.021
@Frequency 1e+6 Hz
Dry; IEC 60250
 0.19
@Frequency 100 Hz
Conditioned; IEC 60250
 0.19
@Frequency 1e+6 Hz
Conditioned; IEC 60250
Comparative Tracking Index 450 VConditioned; IEC 60112
 450 VDry; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 18.0 µm/m-°C
CTE, linear, Transverse to Flow 65.0 µm/m-°C
Melting Point 220 °CISO 3146
Deflection Temperature at 0.46 MPa (66 psi) 220 °CISO 75
Deflection Temperature at 1.8 MPa (264 psi) 215 °CISO 75
UL RTI, Electrical 130 °C
@Thickness 0.750 mm
UL746B
 130 °C
@Thickness 1.50 mm
UL746B
 130 °C
@Thickness 3.00 mm
UL746B
UL RTI, Mechanical with Impact 90.0 °C
@Thickness 1.50 mm
UL746B
 100 °C
@Thickness 3.00 mm
UL746B
UL RTI, Mechanical without Impact 130 °C
@Thickness 1.50 mm
UL746B
 130 °C
@Thickness 3.00 mm
UL746B
Flammability, UL94 HB
@Thickness 1.50 mm
 HB
@Thickness 3.00 mm
 
Processing PropertiesOriginal ValueComments
Melt Temperature 270 - 290 °C
Mold Temperature 80.0 - 90.0 °C
Drying Temperature 180 °C
@Time 7200 - 14400 sec
Moisture Content <= 0.15 %
Injection Pressure 500 - 1500 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBASF8971 / 254929

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.