MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SABIC LNP™ STAT-KON™ Compound DD0009XP Polycarbonate (PC) (Americas)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LNP STAT-KON DD0009XP compound is based on Polycarbonate (PC) resin containing conductive carbon powder. Added features of this grade include: Electrically Conductive, Flame Retardant.

Features: Flame Retardant,Electrically Conductive

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.30 g/cc0.0470 lb/in³ASTM D792
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.130 %0.130 %23°C/50% RH/24 hrs; ASTM D570
 0.210 %0.210 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/in24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/in24hrs; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 46.0 MPa6670 psi5 mm/min; ASTM D638
 50.0 MPa7250 psi5 mm/min; ISO 527
Tensile Strength, Yield 60.0 MPa8700 psi5 mm/min; ISO 527
 69.0 MPa10000 psi5 mm/min; ASTM D638
Elongation at Break 11 %11 %5 mm/min; ISO 527
 13 %13 %5 mm/min; ASTM D638
Elongation at Yield 4.7 %4.7 %5 mm/min; ASTM D638
 4.7 %4.7 %5 mm/min; ISO 527
Tensile Modulus 2.50 GPa363 ksi1 mm/min; ISO 527
Flexural Modulus 2.52 GPa365 ksi2 mm/min; ISO 178
Izod Impact Notched 136 J100 ft-lbASTM D256
Izod Impact, Unnotched 16.25 J/cm30.44 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 9.00 kJ/m²4.28 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 152 kJ/m²72.3 ft-lb/in²80*10*4; ISO 180/1U
Impact Test 33.0 J24.3 ft-lbMultiaxial Impact; ISO 6603
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 1e+05 - 1.00e+10 ohm1e+05 - 1.00e+10 ohmASTM D257
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 139 °C282 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 140 °C
@Thickness 3.20 mm
284 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 131 °C268 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 132 °C
@Thickness 3.20 mm
270 °F
@Thickness 0.126 in
unannealed; ASTM D648
UL RTI, Electrical 80.0 °C176 °FUL 746B
UL RTI, Mechanical with Impact 80.0 °C176 °FUL 746B
UL RTI, Mechanical without Impact 80.0 °C176 °FUL 746B
Flammability, UL94 V-0
@Thickness 1.70 mm
V-0
@Thickness 0.0669 in
UL 94
 
Processing PropertiesMetricEnglishComments
Zone 2 255 - 265 °C491 - 509 °F
Zone 3 260 - 270 °C500 - 518 °F
Melt Temperature 255 - 290 °C491 - 554 °FInjection Molding
Mold Temperature 40.0 - 65.0 °C104 - 149 °F
Drying Temperature 80.0 °C176 °FInjection Molding
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH81190 / 289137

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.