MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
SABIC NORYL™ Resin N1150 Polyphenylene Ether + PS (PPE+PS) (Asia)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene + Polyphenylene Ether, Unreinforced

Material Notes: NORYL™ N1150 resin is a non-reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This injection moldable grade contains non-brominated, non-chlorinated flame retardant and carries a UL94 flame rating of 5VA at 2.5mm and V0 at 0.75mm. NORYL N1150 resin offers heat resistance, good impact resistance, low specific gravity, and dimensional stability. It is an excellent candidate for a variety of automotive instrument panel applications.

Features: Hydrolytic Stability,Low Creep Sensitivity,Thin Wall,Non-Halogenated,Non-Chlorinated,Non-Brominated,Low Warpage,High Flow,Good Processability

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.11 g/ccASTM D792
Density 1.11 g/ccISO 1183
Moisture Absorption 0.0200 %Injection Molding
Water Absorption at Saturation 0.070 %ISO 62-1
Viscosity 15 cP
@Load 5.00 kg,
Temperature 280 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 15 g/10 min
@Load 5.00 kg,
Temperature 280 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 52.0 MPa50 mm/min; ISO 527
 55.0 MPa50 mm/min; ASTM D638
Tensile Strength, Yield 72.0 MPa50 mm/min; ISO 527
 75.0 MPa50 mm/min; ASTM D638
Elongation at Break 7.0 %50 mm/min; ISO 527
 8.0 %50 mm/min; ASTM D638
Elongation at Yield 3.5 %50 mm/min; ISO 527
 4.0 %50 mm/min; ASTM D638
Tensile Modulus 2650 MPa1 mm/min; ISO 527
 2700 MPa5 mm/min; ASTM D638
Flexural Strength 105 MPayield, 2 mm/min; ISO 178
 117 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2600 MPa2 mm/min; ISO 178
 3050 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 85.0 JASTM D256
 65.0 J
@Temperature -30.0 °C
ASTM D256
Izod Impact, Notched (ISO) 6.00 kJ/m²80*10*4; ISO 180/1A
 4.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Charpy Impact, Notched 6.00 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 40.0 JASTM D3763
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 175 - 250 VUL 746A
Hot Wire Ignition, HWI 15 - 30 sec
@Thickness >=0.750 mm
UL 746A
 30 - 60 sec
@Thickness >=2.00 mm
UL 746A
 60 - 120 sec
@Thickness >=2.50 mm
UL 746A
High Amp Arc Ignition, HAI >= 120 arcs
@Thickness >=0.750 mm
UL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 54.5 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 54.5 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 57.5 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 57.5 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 109 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 108 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 130 °CRate B/50; ASTM D1525
 130 °CRate B/50; ISO 306
 132 °CRate B/120; ISO 306
UL RTI, Electrical 95.0 °CUL 746B
UL RTI, Mechanical with Impact 95.0 °CUL 746B
UL RTI, Mechanical without Impact 95.0 °CUL 746B
Flammability, UL94 V-0
@Thickness >=0.750 mm
UL 94
 5VB
@Thickness >=2.00 mm
UL 94
 5VA
@Thickness >=2.50 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 260 - 290 °C
Zone 2 240 - 280 °C
Zone 3 250 - 290 °C
Melt Temperature 260 - 290 °CInjection Molding
Mold Temperature 70.0 - 95.0 °C
Drying Temperature 95.0 - 100 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 8.00 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa
Shot Size 30 - 70 %
Vent Depth 0.00380 - 0.00510 cm
Screw Speed 20 - 100 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH82355 / 290302

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.