MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Borealis Borcycle™ UJ599MO-71 Polypropylene, 55% Post-consumer Recycled polymer
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: UJ599MO is an integrated virgin/recycled PP solution with 55% post-consumer recyclate content with high melt flow rate, based on Borstar Nucleation Technology that allows cycle time reduction. This grade is intended for injection molding. It is designed for high-speed injection molding and contains nucleating and demolding additives. Products originating from this grade have excellent balance of stiffness and impact strength at ambient and cold temperature, good flow and good demolding properties. 71 refers to color indication _light color_ version of resin UJ599MO. Due to nature of recyclates, some variation in color can be observed between batches. Not intended for use in beverages, drinking water contact, food contact, medical, pharmaceutical or healthcare applications. Available colors: 71 refers to color indication _light color_ version; 90 refers to color indication _white_ version; 99 refers to color indication _natural_ version Cas No. 9010-79-1

Special Features:

  • Good stiffness and impact strength balance
  • Good demolding properties
  • Good flow behavior
Applications:
  • Caps and closures for non-food applications
  • Injection-molded non-food applications

Information provided by Borealis AG

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.910 g/cc0.0329 lb/in³ISO 1183-1
Melt Flow 70.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
70.0 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133-1
Storage Temperature <= 50.0 °C<= 122 °F
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 25.0 MPa3630 psi50 mm/min; ISO 527-2
Elongation at Yield 4.50 %4.50 %50 mm/min; ISO 527-2
Tensile Modulus 1.40 GPa203 ksiISO 527-2
Charpy Impact, Notched 0.550 J/cm²2.62 ft-lb/in²ISO 179-1/1eA
 
Thermal PropertiesMetricEnglishComments
Shrinkage 1.00 - 2.00 %1.00 - 2.00 %
 
Processing PropertiesMetricEnglishComments
Melt Temperature 210 - 260 °C410 - 500 °F
Mold Temperature 30.0 - 40.0 °C86.0 - 104 °F
Hold Pressure 20.0 - 50.0 MPa2900 - 7250 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBORE9643 / 323000

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.