MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

EOS MaragingSteel MS1 DMSL on EOS M 300-4
Categories: Metal; 3D Printing/Additive Manufacturing Metal; Ferrous Metal; Maraging Steel

Material Notes: Parts built with EOS MaragingSteel MS1 are characterized by having very good mechanical properties and being easily heat-treatable using a simple thermal age-hardening process to obtain excellent hardness and strength.

Main Characteristics:

  • The parts are easily post-hardened to more than 50 HRC
  • The parts can be machined, spark-eroded, welded, micro shot-peened, polished and coated
  • Chemical composition corresponding to 18Ni300 and M300
Typical Applications:
  • Injection molding tools & inserts
  • Mechanical engineering parts
Heat treatment procedure by solution treatment at 940 °C (1,724 °F) for 2 hours, air cooling to room temperature, age-hardening at 490 °C (914 °F) for 6 hours, air cooling.

Information provided by EOS GmbH (Electro Optical Systems).

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Porosity 0.050 %0.050 %
Thickness 50.0 microns1.97 milLayer Thickness
Pore Size 90.0 microns3.54 mil
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 1100 MPa160000 psiAs manufactured vertical; EN ISO 6892-1 B10
 1200 MPa174000 psiAs manufactured horizontal; EN ISO 6892-1 B10
 2110 MPa306000 psiHeat treated vertical; EN ISO 6892-1 B10
 2120 MPa307000 psiHeat treated horizontal; EN ISO 6892-1 B10
Tensile Strength, Yield 860 MPa125000 psiAs manufactured vertical; EN ISO 6892-1 B10
 980 MPa142000 psiAs manufactured horizontal; EN ISO 6892-1 B10
 1990 MPa289000 psiHeat treated vertical; EN ISO 6892-1 B10
 2040 MPa296000 psiHeat treated horizontal; EN ISO 6892-1 B10
Elongation at Break 3.0 %3.0 %Heat treated vertical; EN ISO 6892-1 B10
 4.0 %4.0 %Heat treated horizontal; EN ISO 6892-1 B10
 12 %12 %As manufactured vertical; EN ISO 6892-1 B10
 13 %13 %As manufactured horizontal; EN ISO 6892-1 B10
 
Descriptive Properties
Volume rateup to 4 x 5.5 mm³/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

NEOS968 / 280628

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.