MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LNP™ STAT-KON™ Compound DE003Z Polycarbonate (PC) (Americas)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LNP STAT-KON DE003Z compound is based on Polycarbonate (PC) resin containing 15% carbon fiber. Added features of this grade include: Electrically Conductive, Extrusion grade.

Features: High Stiffness,Light-weight Structural,Extrusion Grade,Super Strong (Carbon Fiber Filled),Electrically Conductive

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.26 g/cc1.26 g/ccASTM D792
Density 1.253 g/cc0.04527 lb/in³ASTM D792
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.130 %0.130 %23°C/50% RH/24 hrs; ASTM D570
 0.210 %0.210 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0010 - 0.0030 cm/cm0.0010 - 0.0030 in/in24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0040 - 0.0060 cm/cm0.0040 - 0.0060 in/in24hrs; ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 130 MPa18900 psi5 mm/min; ISO 527
 134 MPa19400 psi5 mm/min; ASTM D638
Tensile Strength, Yield 134 MPa19400 psi5 mm/min; ASTM D638
Elongation at Break 2.4 %2.4 %5 mm/min; ASTM D638
 2.6 %2.6 %5 mm/min; ISO 527
Tensile Modulus 10.66 GPa1546 ksi1 mm/min; ISO 527
 11.32 GPa1642 ksi5 mm/min; ASTM D638
Flexural Strength 191 MPa27700 psiISO 178
 200 MPa29000 psibrk, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 9.12 GPa1320 ksi1.3 mm/min, 50 mm span; ASTM D790
 9.29 GPa1350 ksi2 mm/min; ISO 178
Izod Impact Notched 98.0 J72.3 ft-lbASTM D256
Izod Impact, Unnotched 6.23 J/cm11.7 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 8.00 kJ/m²3.81 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 39.0 kJ/m²18.6 ft-lb/in²80*10*4; ISO 180/1U
Dart Drop, Total Energy 24.0 J17.7 ft-lbASTM D3763
Impact Test 4.00 J2.95 ft-lbMultiaxial Impact; ISO 6603
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 22.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
12.2 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
CTE, linear, Transverse to Flow 48.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
26.7 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 147 °C297 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 147 °C
@Thickness 3.20 mm
297 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 143 °C289 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 144 °C
@Thickness 3.20 mm
291 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Zone 2 310 - 320 °C590 - 608 °F
Zone 3 320 - 330 °C608 - 626 °F
Melt Temperature 305 - 325 °C581 - 617 °FInjection Molding
Mold Temperature 80.0 - 110 °C176 - 230 °F
Drying Temperature 120 °C248 °FInjection Molding
Dry Time 4.00 hour4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH81212 / 289159

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.