MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
SABIC LNP™ LUBRICOMP™ Compound NL001 Polycarbonate + ABS (PC+ABS) (Americas)
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced

Material Notes: LNP LUBRICOMP NL001 compound is based on Polycarbonate / Acrylonitrile Butadiene Styrene (PC/ABS) blend containing 5% PTFE. Added features of this grade include: Wear Resistant, suitable for Thin Wall applications.

Features: Thin Wall,Wear resistant

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.14 g/ccASTM D792
Density 1.10 g/ccISO 1183
Moisture Absorption 0.0200 %Injection Molding
Viscosity 26 cP
@Load 5.00 kg,
Temperature 260 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
SABIC method
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 40.0 MPa5 mm/min; ISO 527
 40.0 MPa50 mm/min; ISO 527
 43.0 MPa50 mm/min; ASTM D638
Tensile Strength, Yield 45.0 MPa5 mm/min; ISO 527
 50.0 MPa50 mm/min; ISO 527
 53.0 MPa50 mm/min; ASTM D638
Elongation at Break 20 %50 mm/min; ISO 527
 24.3 %50 mm/min; ASTM D638
 45 %5 mm/min; ISO 527
Elongation at Yield 3.6 %50 mm/min; ASTM D638
 4.0 %5 mm/min; ISO 527
 4.0 %50 mm/min; ISO 527
Tensile Modulus 2300 MPa1 mm/min; ISO 527
 2400 MPa50 mm/min; ASTM D638
Flexural Strength 80.0 MPayield, 2 mm/min; ISO 178
 86.0 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2440 MPa1.3 mm/min, 50 mm span; ASTM D790
 2500 MPa2 mm/min; ISO 178
Izod Impact Notched 160 JASTM D256
Izod Impact, Notched (ISO) 10.0 kJ/m²80*10*4; ISO 180/1A
 8.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Charpy Impact, Notched 13.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 10.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 42.0 JASTM D3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohmROA; IEC 60093
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 70.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 87.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 114 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 116 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 95.0 °CEdgew 120*10*4 sp=100mm; ISO 75/Ae
 99.0 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 113 °CRate B/50; ISO 306
 115 °CRate B/120; ISO 306
UL RTI, Electrical 60.0 °CUL 746B
UL RTI, Mechanical with Impact 60.0 °CUL 746B
UL RTI, Mechanical without Impact 60.0 °CUL 746B
Flammability, UL94 HB
@Thickness >=0.750 mm
UL 94
Oxygen Index 21 %ISO 4589
 
Processing PropertiesOriginal ValueComments
Zone 2 250 - 260 °C
Zone 3 260 - 270 °C
Melt Temperature 250 - 270 °CInjection Molding
Mold Temperature 40.0 - 80.0 °C
Drying Temperature 80.0 °CInjection Molding
Dry Time 4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa
Screw Speed 30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH80905 / 288852

Proto3000 – 3D Engineering Solutions

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.