MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC LNP™ STAT-KON™ DD0001 PC (Americas)  (Unverified Data**)
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Carbon Fiber Reinforced

Material Notes: LNP STAT-KON* DD0001 is a compound based on Polycarbonate resin containing Carbon Powder. Added features of this material include: Electrically Conductive, Flame Retardant.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.28 g/cc0.0462 lb/in³ASTM D792
Moisture Absorption 0.100 %0.100 %50% RH, 24 hrs; ASTM D570
 0.140 %0.140 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0039 cm/cm0.0039 in/in24 hrs; ISO 294
 0.0040 cm/cm0.0040 in/in24 hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0040 cm/cm0.0040 in/in24 hrs; ASTM D955
 0.0040 cm/cm0.0040 in/in24 hrs; ISO 294
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 64.0 MPa9280 psiASTM D638
 64.0 MPa9280 psiISO 527
Elongation at Break 3.2 %3.2 %ISO 527
 3.6 %3.6 %ASTM D638
Flexural Strength 103 MPa14900 psiISO 178
 116 MPa16800 psiASTM D790
Flexural Modulus 3.51 GPa509 ksiISO 178/1A
 3.52 GPa511 ksiISO 178
Izod Impact, Notched 0.230 J/cm0.431 ft-lb/inASTM D256
Izod Impact, Unnotched 5.50 J/cm10.3 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 2.00 kJ/m²0.952 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 36.0 kJ/m²17.1 ft-lb/in²80*10*4; ISO 180/1U
Instrumented Impact Energy at Peak 1.00 J0.738 ft-lbASTM D3763
Tangent Modulus 3450 MPa500000 psi50 mm/min; ASTM D638
 3750 MPa544000 psi1 mm/min; ISO 527
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 100 - 1.00e+6 ohm100 - 1.00e+6 ohmASTM D257
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  52.2 µm/m-°C
@Temperature -40.0 - 40.0 °C
29.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E 831
 52.2 µm/m-°C
@Temperature -40.0 - 40.0 °C
29.0 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow  52.3 µm/m-°C
@Temperature -40.0 - 40.0 °C
29.1 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E 831
 52.4 µm/m-°C
@Temperature -40.0 - 40.0 °C
29.1 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 88.0 °C190 °FFlatw 80*10*4 sp=64mm; ISO 75/Bf
 86.0 °C
@Thickness 3.20 mm
187 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 82.0 °C180 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 82.0 °C
@Thickness 3.20 mm
180 °F
@Thickness 0.126 in
unannealed; ASTM D648
Flammability, UL94 V-0
@Thickness 1.70 mm
V-0
@Thickness 0.0669 in
UL 94 by SABIC-IP
 
Processing PropertiesMetricEnglishComments
Zone 1 250 - 260 °C482 - 500 °F
Zone 2 255 - 265 °C491 - 509 °F
Zone 3 260 - 270 °C500 - 518 °F
Melt Temperature 255 - 290 °C491 - 554 °F
Mold Temperature 40.0 - 65.0 °C104 - 149 °F
Drying Temperature 80.0 °C176 °F
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hour
Moisture Content 0.020 %0.020 %
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI22242 / 215378

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.