MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
SABIC LEXAN™ Homopolymer 123M PC (Americas)  (Unverified Data**)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: Nonhalogenated. 17.5 MFR, for small, intricate parts. UV stabilized. Improved Internal mold release.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.20 g/ccASTM D792
 1.204 g/ccASTM D792
Density 1.19 g/ccASTM D792
Water Absorption 0.15 %
@Time 86400 sec
ASTM D570
Moisture Absorption at Equilibrium 0.35 %ASTM D570
 0.58 %
@Temperature 100 °C
ASTM D570
Linear Mold Shrinkage, Flow 0.0050 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 17.5 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 66.0 MPaType I, 50. mm/min; ASTM D638
Tensile Strength, Yield 63.0 MPaType I, 50 mm/min; ASTM D638
Elongation at Break 120 %Type I, 50 mm/min; ASTM D638
Elongation at Yield 7.0 %Type I, 50 mm/min; ASTM D638
Flexural Yield Strength 100 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2350 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 820 J/mASTM D256
 200 J/m
@Temperature -30.0 °C
ASTM D256
Izod Impact, Unnotched 2140 J/mASTM D4812
Dart Drop, Total Energy 169 JASTM D3029
Instrumented Impact Total Energy 77.0 JASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 63.6 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E 831
CTE, linear, Transverse to Flow 65.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E 831
Specific Heat Capacity 1.26 J/g-°CASTM C 351
Thermal Conductivity 0.190 W/m-KASTM C177
Deflection Temperature at 0.46 MPa (66 psi) 137 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 132 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 143 °CRate B/50; ASTM D1525
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.586ASTM D542
Haze 1.0 %
@Thickness 2.54 mm
ASTM D1003
Transmission, Visible 88 %
@Thickness 2.54 mm
ASTM D1003
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 275 - 300 °C
Zone 1 260 - 280 °C
Zone 2 270 - 295 °C
Zone 3 280 - 305 °C
Melt Temperature 280 - 305 °C
Mold Temperature 70.0 - 95.0 °C
Drying Temperature 120 °C
Dry Time 3.00 - 4.00 hour
 48.0 hourCumulative
Moisture Content 0.020 %
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 60 %
Vent Depth 0.00250 - 0.00760 cm
Screw Speed 40 - 70 rpm

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Alclad Aluminum 6061-O

PSABI20169 / 213305

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.