SABIC LNP™ THERMOCOMP™ Compound WX05456 Polybutylene Terephthalate (PBT)
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polybutylene Terephthalate (PBT)
;
Polybutylene Terephthalate (PBT), Unreinforced, Molded
Material Notes:
LNP THERMOCOMP WX05456 compound is based on Polybutylene Terephthalate (PBT) resin containing mineral. Added features of this grade include: Low Warpage, Flame Retardant.
Features: Flame Retardant,Low Warpage,Structural
Information provided by SABIC
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.54
g/cc
0.0556
lb/in³
ISO 1183
1.546
g/cc
0.05585
lb/in³
ASTM D792
Moisture Absorption
0.0200 %
0.0200 %
Injection Molding
0.0500 %
0.0500 %
23°C/50% RH/24 hrs; ASTM D570
0.0700 %
0.0700 %
23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow
0.0147
cm/cm
0.0147
in/in
24hrs; ISO 294
0.015
cm/cm
0.015
in/in
24hrs; ASTM D955
Linear Mold Shrinkage, Transverse
0.015
cm/cm
0.015
in/in
24hrs; ASTM D955
0.0151
cm/cm
0.0151
in/in
24hrs; ISO 294
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
47.0
MPa
6820
psi
ISO 527
48.0
MPa
6960
psi
ASTM D638
Elongation at Break
1.4 %
1.4 %
ISO 527
1.8 %
1.8 %
ASTM D638
Tensile Modulus
4.22
GPa
612
ksi
50 mm/min; ASTM D638
4.65
GPa
674
ksi
1 mm/min; ISO 527
Flexural Strength
88.0
MPa
12800
psi
ISO 178
90.0
MPa
13100
psi
ASTM D790
Flexural Modulus
4.20
GPa
609
ksi
ISO 178
4.39
GPa
637
ksi
ASTM D790
Izod Impact Notched
26.0
J
19.2
ft-lb
ASTM D256
Izod Impact, Unnotched
1.97
J/cm
3.69
ft-lb/in
ASTM D4812
Izod Impact, Notched (ISO)
2.00
kJ/m²
0.952
ft-lb/in²
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO)
15.0
kJ/m²
7.14
ft-lb/in²
80*10*4; ISO 180/1U
Dart Drop, Total Energy
7.00
J
5.16
ft-lb
peak; ASTM D3763
Electrical Properties
Metric
English
Comments
Arc Resistance
60
-
120
sec
60
-
120
sec
ASTM D495
Comparative Tracking Index
175
-
250
V
175
-
250
V
UL 746A
Hot Wire Ignition, HWI
15
-
30
sec
@Thickness >=1.50 mm
15
-
30
sec
@Thickness >=0.0591 in
UL 746A
30
-
60
sec
@Thickness >=3.00 mm
30
-
60
sec
@Thickness >=0.118 in
UL 746A
High Amp Arc Ignition, HAI
15
-
30
arcs
@Thickness >=1.50 mm
15
-
30
arcs
@Thickness >=0.0591 in
UL 746A
High Voltage Arc-Tracking Rate, HVTR
10.0
-
25.4
mm/min
0.394
-
1.00
in/min
UL 746A
Thermal Properties
Metric
English
Comments
CTE, linear, Parallel to Flow
58.1
µm/m-°C
@Temperature -40.0 - 40.0 °C
32.3
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
58.1
µm/m-°C
@Temperature -40.0 - 40.0 °C
32.3
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow
66.7
µm/m-°C
@Temperature -40.0 - 40.0 °C
37.1
µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
66.8
µm/m-°C
@Temperature -40.0 - 40.0 °C
37.1
µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi)
163
°C
325
°F
Flatw 80*10*4 sp=64mm; ISO 75/Bf
171
°C
@Thickness 3.20 mm
340
°F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
82.0
°C
180
°F
Flatw 80*10*4 sp=64mm; ISO 75/Af
71.0
°C
@Thickness 3.20 mm
160
°F
@Thickness 0.126 in
unannealed; ASTM D648
UL RTI, Electrical
105
°C
221
°F
UL 746B
UL RTI, Mechanical with Impact
105
°C
221
°F
UL 746B
UL RTI, Mechanical without Impact
105
°C
221
°F
UL 746B
Flammability, UL94
V-0
@Thickness >=1.50 mm
V-0
@Thickness >=0.0591 in
UL 94
Processing Properties
Metric
English
Comments
Zone 2
250
-
260
°C
482
-
500
°F
Zone 3
265
-
275
°C
509
-
527
°F
Melt Temperature
250
-
275
°C
482
-
527
°F
Injection Molding
Mold Temperature
80.0
-
95.0
°C
176
-
203
°F
Drying Temperature
120
-
150
°C
248
-
302
°F
Injection Molding
Dry Time
4.00
hour
4.00
hour
Injection Molding
Back Pressure
0.200
-
0.300
MPa
29.0
-
43.5
psi
Screw Speed
30
-
60
rpm
30
-
60
rpm
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PSABH81963 / 289910
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.