MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Syensqo (Solvay Specialty Polymers) KetaSpire® KT-880 CF40 PEEK, 40% carbon fiber
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Carbon Fiber Filled

Material Notes: KetaSpire® KT-880 CF40 is a 40% chopped carbon fiber-reinforced polyetheretherketone (PEEK.) The carbon fiber content in the formulation is designed to provide maximum strength and stiffness properties in a filled PEEK compound. The resin enjoys all the key performance attributes for which PEEK is known including resistance to harsh chemical environments, high heat resistance (both short and long term), along with excellent fatigue resistance.

This resin is a high flowing/low viscosity grade and is ideally suited for use in injection molding fabrication. It can be melt processed using standard thermoplastic melt processing equipment.

Potential application areas for KT-880 CF40 include uses in the aerospace industry and some other transportation applications where maximum mechanical properties are desired while maintaining a low specific gravity. Semiconductor fabrication is another industrial area of possible use for this resin as are the chemical processing, oil and gas, and health care industries.

Applications: Aircraft Applications; Connectors; Dental Applications; Electrical/Electronic Applications; Film; Hospital Goods; Industrial Applications; Medical Devices; Medical/Healthcare Applications; Oil/Gas Applications; Pump Parts; Seals; Surgical Instruments

Features: Autoclave Sterilizable; Chemical Resistant; E-beam Sterilizable; Ethylene Oxide Sterilizable; Fatigue Resistant; Flame Retardant; Good Dimensional Stability; Good Sterilizability; Heat Sterilizable; High Flow; High Heat Resistance; High Stiffness; High Strength; Radiation (Gamma) Resistant; Radiation Sterilizable; Radiotranslucent; Steam Resistant; Steam Sterilizable

Information provided by Solvay Specialty Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.46 g/cc0.0527 lb/in³ASTM D792
Viscosity 490 cP
@Shear Rate 1000 1/s,
Temperature 400 °C
490 cP
@Shear Rate 1000 1/s,
Temperature 752 °F
Melt; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 258 MPa37400 psiASTM D638
Elongation at Break 1.6 %1.6 %5.0 mm/min; ASTM D638
Tensile Modulus 33.0 GPa4790 ksiASTM D638
Flexural Strength 386 MPa56000 psiASTM D790
Flexural Modulus 30.0 GPa4350 ksiASTM D790
Izod Impact, Notched 0.800 J/cm1.50 ft-lb/inASTM D256
Izod Impact, Unnotched 7.50 J/cm14.1 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 332 °C630 °FAnnealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 365 °C689 °F
Middle Barrel Temperature 370 °C698 °F
Front Barrel Temperature 375 °C707 °F
Nozzle Temperature 380 °C716 °F
Mold Temperature 175 - 205 °C347 - 401 °F
Drying Temperature 150 °C
@Time 14400 sec
302 °F
@Time 4.00 hour
 
Descriptive Properties
AvailabilityAsia Pacific
 Europe
 Latin America
 North America
ColorBlack
FormsPellets
Injection RateFast
ProcessingInjection Molding; Machining; Profile Extrusion
Screw Compression Ratio2.5:1.0 to 3.5:1.0

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSOL8Y4336 / 280136

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.