Physical Properties | Metric | English | Comments |
---|
Density | 2.40 g/cc | 0.0867 lb/in³ |
Thickness | 400 - 1200 microns | 15.7 - 47.2 mil |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Vickers | 590 | 590 |
| 651 | 651 |
Modulus of Elasticity | 77.0 GPa | 11200 ksi |
Poissons Ratio | 0.22 | 0.22 |
Fracture Toughness | 0.760 MPa-m½ | 0.692 ksi-in½ |
Shear Modulus | 31.4 GPa | 4550 ksi |
|
Electrical Properties | Metric | English | Comments |
---|
Dielectric Constant | 6.74 @Frequency 4.90e+8 Hz | 6.74 @Frequency 4.90e+8 Hz |
| 6.74 @Frequency 5.99e+8 Hz | 6.74 @Frequency 5.99e+8 Hz |
| 6.75 @Frequency 3.81e+8 Hz | 6.75 @Frequency 3.81e+8 Hz |
| 6.76 @Frequency 2.986e+9 Hz | 6.76 @Frequency 2.986e+9 Hz |
| 6.77 @Frequency 2.72e+8 Hz | 6.77 @Frequency 2.72e+8 Hz |
| 6.78 @Frequency 1.63e+8 Hz | 6.78 @Frequency 1.63e+8 Hz |
| 6.78 @Frequency 1.977e+9 Hz | 6.78 @Frequency 1.977e+9 Hz |
| 6.78 @Frequency 2.466e+9 Hz | 6.78 @Frequency 2.466e+9 Hz |
| 6.8 @Frequency 1.499e+9 Hz | 6.8 @Frequency 1.499e+9 Hz |
| 6.81 @Frequency 9.12e+8 Hz | 6.81 @Frequency 9.12e+8 Hz |
| 6.82 @Frequency 5.40e+7 Hz | 6.82 @Frequency 5.40e+7 Hz |
Dissipation Factor | 0.0080 @Frequency 5.40e+7 Hz | 0.0080 @Frequency 5.40e+7 Hz |
| 0.0080 @Frequency 1.63e+8 Hz | 0.0080 @Frequency 1.63e+8 Hz |
| 0.0090 @Frequency 2.72e+8 Hz | 0.0090 @Frequency 2.72e+8 Hz |
| 0.0090 @Frequency 3.81e+8 Hz | 0.0090 @Frequency 3.81e+8 Hz |
| 0.0090 @Frequency 4.90e+8 Hz | 0.0090 @Frequency 4.90e+8 Hz |
| 0.0090 @Frequency 5.99e+8 Hz | 0.0090 @Frequency 5.99e+8 Hz |
| 0.010 @Frequency 9.12e+8 Hz | 0.010 @Frequency 9.12e+8 Hz |
| 0.011 @Frequency 1.499e+9 Hz | 0.011 @Frequency 1.499e+9 Hz |
| 0.011 @Frequency 1.977e+9 Hz | 0.011 @Frequency 1.977e+9 Hz |
| 0.012 @Frequency 2.466e+9 Hz | 0.012 @Frequency 2.466e+9 Hz |
| 0.012 @Frequency 2.986e+9 Hz | 0.012 @Frequency 2.986e+9 Hz |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 7.52 µm/m-°C @Temperature 0.000 - 300 °C | 4.18 µin/in-°F @Temperature 32.0 - 572 °F |
Softening Point | 884.9 °C | 1625 °F |
Annealing Point | 624 °C | 1160 °F |
Strain Point | 572 °C | 1060 °F |
|
Optical Properties | Metric | English | Comments |
---|
Refractive Index | 1.50 @Wavelength 590 nm | 1.50 @Wavelength 590 nm |
| 1.51 @Wavelength 590 nm | 1.51 @Wavelength 590 nm |
Transmission, Visible | >= 90.5 % @Wavelength 380 - 2000 nm, Thickness 0.700 mm | >= 90.5 % @Wavelength 380 - 2000 nm, Thickness 0.0276 in |
IR Transmittance | >= 90.5 % @Wavelength 380 - 2000 nm, Thickness 0.700 mm | >= 90.5 % @Wavelength 380 - 2000 nm, Thickness 0.0276 in |
|
Descriptive Properties |
---|
Photo-elastic Constant | 30.6 nm/cm/MPa |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding