MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Momentive Performance Materials GE Silicones SCS1200 Acetoxy Silicone Construction Sealant
Categories: Polymer; Thermoset; Silicone

Material Notes: GE SCS1200 construction silicone glazing sealant is a one-component, high strength, acetoxy silicone adhesive for structural, butt joint and general purpose glazing applications. The material is supplied as a paste, which cures into a durable rubber when exposed to atmospheric moisture.

Features: Silicone Durability, Fast Cure Time, Primerless Adhesion, High Tensile Strength, ±25% Movement Capacity, Stable Consistency (uncured), Cured Thermal Stability, Low Sag or Slump.

Applications: SCS1200 construction silicone glazing sealant is a candidate to consider in structural glazing applications. It may be used as a weather seal product for general purpose glazing, butt glazing and for tall glass-stiffened lobby systems. SCS1200 sealant has been successfully tested in protective glazing applications and may be considered a candidate for such applications. SCS1200 sealant may be considered for sealing air conditioning, vents or other wall penetrations; glass block, metal/plastic signs or marine hardware.

Colors: Translucent(SCS1201), White(SCS1202), Black(SCS1203), Aluminum-metallic(SCS1209), Bronze(SCS1297).

Information provided by Momentive Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Volatile Organic Compounds (VOC) Content 23 g/lUncured; WPSTM C1454
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 28ASTM D2240
Tensile Strength, Ultimate 3.31 MPaASTM D412
Elongation, Ultimate 513 %ASTM D412
Shear Strength 0.760 MPa
@Thickness 6.35 mm
ASTM C961
Tear Strength 8.07 kg(f)/cmDie B.; ASTM D624
Peel Strength 10.89 pli
@Temperature 23.9 °C,
Time 1.81e+6 sec
50%RH; ASTM C794
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 400 °F
Minimum Service Temperature, Air -55.0 °F
 
Processing PropertiesOriginal ValueComments
Cure Time 120 - 168 hourFull cured. Common applications.
 24.0 hour
@Temperature 24.0 °C
1/4" deep section. 50% RH
Tack-Free Time 30.0 min
@Temperature 23.9 °C
50% RH; ASTM C679
Working Life 5.00 - 10.0 min
 
Descriptive Properties
AppearancePaste
Consistency / Sag0.1" maxASTM D2202
Joint Movement Capability+/- 25%ASTM C719.
Silicone Content (%)100Uncured
UV & Weathering ResistanceExcellentGE 20 yr study

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PMOMEN9919 / 265729

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.