MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Crosspolimeri POLIGOM G/44 EPR/EPDM
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: POLIGOM: is the trade-mark of our flexible crosslinkable EPR/EPDM polymer.

POLIGOM G/44: chemically crosslinkable elastomer base for low voltage cable insulation and sheathing. It is a conveniently grafted compound able to react in presence of moisture and of a catalyst. We normally suggest our catalyst type MAC/100 SCU or MAC/600 P2 (flexible type). REACTION BETW EEN GRAFTING AND CATALYST: These two com pounds, separately stored, must be mixed before starting extrusion in the ratio: GRAFTING/CATALYST 94/6

Certify: HD 22, 1 EI4-EI6-EI7-EM3, VDE 0207/20 3GI3, BS 7655 RS5-GP7

Information provided by Crosspolimeri S.P.A.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.880 g/ccASTM D792
Melt Flow 4.0 - 7.0 g/10 min
@Load 5.00 kg,
Temperature 190 °C
ASTM D1238
Storage Temperature 12.0 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 67ASTM D2240
Tensile Strength 10.0 MPaIEC 60811
 10.7 MPa
@Temperature 135 °C,
Time 605000 sec
Heat Ageing; IEC 60811
Elongation at Break 450 %IEC 60811
 495 %
@Temperature 135 °C,
Time 605000 sec
Heat Ageing; IEC 60811
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 4.00e+15 ohm-cmIEC 60502
Dielectric Strength 32.0 kV/mmASTM D149
 
Processing PropertiesOriginal ValueComments
Zone 1 130 °C
Zone 2 140 °C
Zone 3 160 °C
Zone 4 170 °C
Die Temperature 175 °C
Head Temperature 170 °C
 
Descriptive Properties
Hot Set Test0Residual Value, IEC 811
 0.7250°C - 20 N/cm2, IEC 811

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PCROS134 / 294218

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.