MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

BASF Ultramid® A 218 V40 Black 21N Nylon 66, 40% Glass Fiber Reinforced, Heat Stabilized, Dry
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 40% Glass Fiber Filled; Nylon 66, Heat Stabilized

Material Notes: Product Description: Ultramid® A 218 V40 Black 21N is a polyamide 66, reinforced with 40% of glass fiber, heat stabilized, for injection molding. This grade offers an excellent combination between thermal and mechanical properties.

Availability: Africa & Middle East; Asia Pacific; Latin America; North America

Filler/Reinforcement: Glass Fiber, 40% Filler by Weight

Features: Good Dimensional Stability; Good Flow; Good Mold Release; Heat Stabilized – Inorganic

Use: Automotive Applications

Agency Ratings: EC 1907/2006 (REACH)

RoSH Compliance: RoSH Compliant

Appearance: Black

Forms: Pellets

Processing Method: Injection Molding

Resin ID (ISO 1043): PA66-GF40

Information provided by BASF Corporation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.46 g/cc0.0527 lb/in³ISO 1183
Water Absorption 1.9 %1.9 %Equilibrium, 50% RH; ISO 62
 0.70 %
@Time 86400 sec
0.70 %
@Time 24.0 hour
ISO 62
Maximum Moisture Content 0.200.20
Linear Mold Shrinkage, Flow 0.0090 cm/cm0.0090 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0035 cm/cm0.0035 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 215 MPa31200 psiISO 527-2
Elongation at Break 2.5 %2.5 %ISO 527-2
Tensile Modulus 13.0 GPa1890 ksiISO 527-1
Flexural Modulus 11.0 GPa1600 ksiISO 178
Izod Impact, Notched (ISO) 13.4 kJ/m²6.40 ft-lb/in²ISO 180/A
Charpy Impact Unnotched 8.40 J/cm²40.0 ft-lb/in²ISO 179/1eU
Charpy Impact, Notched 1.49 J/cm²7.10 ft-lb/in²ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+15 ohm-cm1.00e+15 ohm-cmIEC 62631-3-1
Dielectric Constant 3.7
@Frequency 100 Hz
3.7
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 35.0 kV/mm
@Thickness 2.00 mm
890 kV/in
@Thickness 0.0787 in
IEC 60243-1
Dissipation Factor 0.010
@Frequency 100 Hz
0.010
@Frequency 100 Hz
IEC 62631-2-1
Comparative Tracking Index 400 V400 VSolution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 262 °C504 °FISO 11357-3
Deflection Temperature at 1.8 MPa (264 psi) 255 °C491 °FUnannealed; ISO 75-2/A
Flammability, UL94 HB
@Thickness 1.52 mm
HB
@Thickness 0.0600 in
IEC 60695-11-10,-20
Oxygen Index 23 %23 %ISO 4589-2
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 270 - 280 °C518 - 536 °F
Middle Barrel Temperature 280 - 290 °C536 - 554 °F
Front Barrel Temperature 280 - 300 °C536 - 572 °F
Mold Temperature 70.0 - 100 °C158 - 212 °F
Drying Temperature 80.0 °C176 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBASG2092 / 310785

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.