System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Kumho-Sunny H2938Z ABS, Heat Resistance
Categories:
Polymer
;
Thermoplastic
;
ABS Polymer
;
Acrylonitrile Butadiene Styrene (ABS), Heat Resistant, Molded
Material Notes:
ABSH2938Z is heat resistance ABS with low gloss, high rigidity, toughness and good UV stability.
Application: Hair dryer shells, electric oven exterior parts and microwave ovens etc.
Information provided by Shanghai Kumho Sunny Plastics co, Ltd
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
1.05
g/cc
ISO 1183
Maximum Moisture Content
0.050
Linear Mold Shrinkage
0.0040
-
0.0070
cm/cm
ISO 294
Melt Flow
12
g/10 min
@Load 10.0 kg,
Temperature 220 °C
ISO 1133
Mechanical Properties
Original Value
Comments
Hardness, Rockwell R
106
ISO 2039-2
Tensile Strength
45.0
MPa
50mm/min; ISO 527
Elongation at Break
25 %
50mm/min; ISO 527
Flexural Strength
65.0
MPa
2mm/min; ISO 178
Flexural Modulus
2300
MPa
2mm/min; ISO 178
Poissons Ratio
0.38
1mm/min; ISO 527
Izod Impact, Notched (ISO)
9.00
kJ/m²
@Temperature -30.0 °C
5.5J; ISO 180
17.0
kJ/m²
@Temperature 23.0 °C
5.5J; ISO 180
Izod Impact, Unnotched (ISO)
NB
5.5J; ISO 180
Charpy Impact Unnotched
NB
4J; ISO 179
Charpy Impact, Notched
10.0
kJ/m²
@Temperature 23.0 °C
4J; ISO 179
18.0
kJ/m²
@Temperature -30.0 °C
4J; ISO 179
Electrical Properties
Original Value
Comments
Volume Resistivity
>=
1.00e+15
ohm-cm
IEC 60093
Surface Resistance
>=
1.00e+15
ohm
IEC 60093
Thermal Properties
Original Value
Comments
Deflection Temperature at 0.46 MPa (66 psi)
100
°C
120°C/h; ISO 75
Deflection Temperature at 1.8 MPa (264 psi)
85.0
°C
120°C/h; ISO 75
Vicat Softening Point
104
°C
@Load 5.00 kg
50°C/h; ISO 306
Flammability, UL94
HB
Processing Properties
Original Value
Comments
Rear Barrel Temperature
190
-
210
°C
Middle Barrel Temperature
210
-
220
°C
Front Barrel Temperature
220
-
235
°C
Nozzle Temperature
230
-
245
°C
Melt Temperature
230
-
250
°C
Mold Temperature
50.0
-
80.0
°C
Drying Temperature
80.0
-
90.0
°C
Dry Time
3.00
-
4.00
hour
Back Pressure
1.00
-
5.00
MPa
Screw Speed
30
-
70
rpm
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
PKMSN035 / 280887
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.