MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Celanese Celanex® 2008 PBT  (Unverified Data**)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: Celanex 2008 is a general purpose, unreinforced polybutylene terephthalate with a good balance of mechanical properties and processability for use in melt blown applications.
Ultrahigh melt flow

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.31 g/ccASTM D792
Density 1.31 g/ccISO 1183
Water Absorption 0.090 %24hr immersion; ASTM D570
Moisture Absorption 0.170 %23°C/50%RH; ISO 62
Linear Mold Shrinkage, Flow 0.018 - 0.020 in/inASTM D955
 0.018 - 0.020 cm/cmISO 294-4
Linear Mold Shrinkage, Transverse 0.018 - 0.020 cm/cmISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 72ISO 2039-2
Tensile Strength at Break 47.0 MPa50mm/min; ISO 527-2/1A
 60.0 MPa5mm/min; ISO 527-2/1A
Tensile Strength, Yield 8000 psiASTM D638
Elongation at Break 2.0 %50mm/min; ISO 527-2/1A
 5.0 %5mm/min; ISO 527-2/1A
 5.0 %
@Temperature 22.8 °C
ASTM D638
Tensile Modulus 2600 MPa1mm/min; ISO 527-2/1A
Flexural Strength 80.0 MPaISO 178
 12000 psiASTM D790
Flexural Modulus 2200 MPaISO 178
 330000 psi
@Temperature 22.8 °C
ASTM D790
Izod Impact, Notched 0.500 ft-lb/inASTM D256
Izod Impact, Notched (ISO) 3.10 kJ/m²ISO 180/1A
Charpy Impact Unnotched 38.0 kJ/m²ISO 179/1eU
 44.0 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
Charpy Impact, Notched 2.80 kJ/m²ISO 179/1eA
 2.10 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093
 1.00e+16 ohm-cmASTM D257
Surface Resistance >= 1.00e+15 ohmIEC 60093
Dielectric Constant 3.2
@Frequency 1e+6 Hz
ASTM D150
 3.2
@Frequency 1e+6 Hz
IEC 60250
 3.3
@Frequency 100 Hz
IEC 60250
Dielectric Strength 15.0 kV/mmIEC 60243-1
 400 V/milshort term; ASTM D149
Dissipation Factor 0.0010
@Frequency 1e+6 Hz
ASTM D150
 0.020
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 350 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 110 µm/m-°CISO 11359-2
CTE, linear, Transverse to Flow 100 µm/m-°CISO 11359-2
Melting Point 225 °C10°C/min; ISO 11357-1,-2,-3
 437 °FASTM D3418
Transformation Temperature, Tg 60.0 °C10°C/min; ISO 11357-1,-2,-3
Deflection Temperature at 0.46 MPa (66 psi) 155 °CISO 75-1, -2
 310 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 57.0 °CISO 75-1, -2
 130 °FASTM D648
Flammability, UL94 HBUL94
 
Processing PropertiesOriginal ValueComments
Processing Temperature 20.0 - 50.0 °C
 65.0 - 93.0 °CCavity temperature
Feed Temperature 230 - 240 °C
Rear Barrel Temperature 230 - 240 °C
Middle Barrel Temperature 235 - 250 °C
Front Barrel Temperature 240 - 260 °C
Nozzle Temperature 250 - 260 °C
Zone 1 230 - 240 °C
Zone 2 235 - 250 °C
Zone 3 235 - 250 °C
Zone 4 240 - 260 °C
Die Temperature 250 - 260 °C
Melt Temperature 243 °CInjection molding; ISO 294
 235 - 260 °C
Mold Temperature 82.0 °CInjection molding; ISO 294
 150 - 200 °F
Injection Velocity 300 mm/secISO 294
Drying Temperature 120 - 130 °C
Dry Time 4.00 hour
Moisture Content 0.020 %Necessary low maximum residual
Hold Pressure 48.0 MPaISO 294
Back Pressure 0.000 - 50.0 psi
Hot-Working Temperature 250 - 260 °C
 
Descriptive Properties
Injection moldingYes
Injection speedmedium-fast
Longer pre-drying times/storagelower the temperature to 100° C until processed.<= 60 h
Processing conditionsISO 7792-2
Processing NotesFast Injection Speed
 Medium Screw Speed

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHCR018 / 158585

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.