MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Arkema Elium® 591 SO Thermoplastic Resin for Composites
Categories: Polymer; Thermoplastic

Material Notes: This grade is suggested for automotive, wind, and industrial uses.

Elium® is a liquid thermoplastic resin designed for manufacturing composite parts with mechanical properties similar to thermosets. The major advantage of Elium® is it acts like a thermoplastic, which means it is uniquely designed for thermoforming, recycling, and welding.

Elium® resins are processed on similar equipment to that used for thermoset composites, with similar polymerization cycle times and conditions.

Information provided by Arkema.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Viscosity 500 cP500 cP
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 85 - 9085 - 90ISO 868
Tensile Strength 66.0 MPa9570 psiISO 527
Elongation at Break 2.8 %2.8 %ISO 527
Tensile Modulus 3.17 GPa460 ksiISO 527
Flexural Strength 111 MPa16100 psiISO 178
Flexural Modulus 2.91 GPa422 ksiISO 178
Compressive Strength 116 MPa16800 psiISO 14126
Compressive Modulus 3.83 GPa556 ksiISO 14126
Fracture Toughness 1.20 MPa-m½1.09 ksi-in½KIC; ISO 13586
 
Thermal PropertiesMetricEnglishComments
CTE, linear 65.0 µm/m-°C36.1 µin/in-°FISO 2155-1
 
Processing PropertiesMetricEnglishComments
Processing Temperature 20.0 - 115 °C68.0 - 239 °FAdjustable
 
Descriptive Properties
Example PeroxidePeroxide Blend
ProcessPultrusion
 Wet Compressing
 Winding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PARKF006 / 265388

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.