MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Ascend Performance Materials HiDura™ PTR 840F Nylon PA66/6
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6/66; Nylon 66/6, Unreinforced

Material Notes: HiDura PTR 840F is a polyamide copolymer that features good melt strength, flexibility, toughness, and slow crystallization. It offers melt viscosity and crystallization rate suitable for blown film, multi-bubble blown film, and thermoforming.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.12 g/ccDAM; ISO 1183
Water Absorption 3.2 %
@Time 86400 sec
DAM; ISO 62
Moisture Absorption <= 0.100 %ASTM D 6869
Moisture Absorption at Equilibrium 2.7 %DAM to 50% RH; ISO 62
Water Absorption at Saturation 11 %ISO 62
Viscosity Measurement 3.9Relative Viscosity; Sulfuric Acid; ISO 307
Linear Mold Shrinkage, Flow 0.014 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
Linear Mold Shrinkage, Transverse 0.014 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 64.0 MPa50% RH; ISO 527-2
 70.0 MPaDAM; ISO 527-2
Elongation at Break 212 %DAM; ISO 527-2
 386 %50% RH; ISO 527-2
Tensile Modulus 627 MPa50% RH; ISO 527-2
 2300 MPaDAM; ISO 527-2
Flexural Strength 14.0 MPa50% RH; ISO 178
 74.0 MPaDAM; ISO 178
Flexural Modulus 476 MPa50% RH; ISO 178
 2400 MPaDAM; ISO 178
Izod Impact, Notched (ISO) 4.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 4.20 kJ/m²
@Temperature -40.0 °C
DAM; ISO 180/1A
 4.30 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 4.80 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 180/1A
 5.80 kJ/m²
@Temperature -40.0 °C
50% RH; ISO 180/1A
 17.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 180/1A
Charpy Impact Unnotched 164 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eU
 178 kJ/m²
@Temperature -40.0 °C
50% RH; ISO 179/1eU
 179 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eU
 NB
@Temperature -40.0 °C
DAM; ISO 179/1eU
 NB
@Temperature -30.0 °C
DAM; ISO 179/1eU
 NB
@Temperature 23.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 2.60 kJ/m²
@Temperature -30.0 °C
50% RH; ISO 179/1eA
 2.70 kJ/m²
@Temperature -40.0 °C
50% RH; ISO 179/1eA
 3.20 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eA
 3.30 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 3.80 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 42.0 kJ/m²
@Temperature 23.0 °C
50% RH; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 28.0 kV/mm
@Thickness 1.00 mm
50% RH; IEC 60243
 28.0 kV/mm
@Thickness 1.00 mm
DAM; IEC 60243
 
Thermal PropertiesOriginal ValueComments
Melting Point 227 °CDAM; ISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 69.0 °CUnannealed; DAM; ISO 75-2/B
 120 °CUnannealed; 50% RH; ISO 75-2/B
Deflection Temperature at 1.8 MPa (264 psi) 47.0 °CUnannealed; DAM; ISO 75-2/A
 71.0 °CUnannealed; 50% RH; ISO 75-2/A
 
Processing PropertiesOriginal ValueComments
Zone 1 245 - 265 °CExtrusion
Zone 2 245 - 265 °CExtrusion
Zone 3 240 - 260 °CExtrusion
Zone 4 230 - 255 °CExtrusion
Zone 5 225 - 250 °CExtrusion
Die Temperature 245 - 265 °CExtrusion
Melt Temperature 245 - 265 °CExtrusion
 
Descriptive Properties
AdditiveLubricant
Agency RatingsASTM, D4066
 ASTM, D6779
 EC, 1935/2004
 EU, 10/2011
 EU, 2023/2006
 FDA, 21 CFR 177.1500
AppearanceNatural Color
FeaturesChemical Resistant
 High Elongation
 High Impact Resistance
 High Melt Stability
 High Melt Strength
 High Strength
 High Toughness
 High Viscosity
 Lubricated
 Puncture Resistant
FormsPellets
RegionNorth America, Europe, Asia Pacific

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PASCE8606 / 293355

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.