MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Pressure Seal 8782 Fluorinated Hydrocarbon
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 8782 is a 75 durometer black colored Viton® GF-S elastomer that is peroxide cured. It exhibits excellent resistance to a wide variety of chemicals including concentrated acids.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 HK 820 A1-10 B37 B38 EF31 EO78 F15 Z1; 4 HK 820 A1-11 B38 EF31 EO78 Z1; 6 HK 820 A1-10 A1-11 B31 B38 EO88 F15 Z1
Z1 = 75 ± 5 Shore A Durometer

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.92 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 77
 68
@Temperature 23.0 °C,
Time 7.20e+6 sec
Concentrated Nitric Acid
 69
@Temperature 23.0 °C,
Time 5.76e+6 sec
50% MeOH/50% FUEL C
 69
@Temperature 23.0 °C,
Time 2.16e+6 sec
50% MeOH/50% FUEL C
 70
@Temperature 23.0 °C,
Time 605000 sec
50% MeOH/50% FUEL C
 71
@Temperature 23.0 °C,
Time 5.76e+6 sec
15% EtOH/85% FUEL C
 72
@Temperature 23.0 °C,
Time 252000 sec
50% MeOH/50% FUEL C
 72
@Temperature 23.0 °C,
Time 2.16e+6 sec
15% EtOH/85% FUEL C
 72
@Temperature 200 °C,
Time 252000 sec
Stauffer Blend 7700
 73
@Temperature 23.0 °C,
Time 605000 sec
15% EtOH/85% FUEL C
 73
@Temperature 23.0 °C,
Time 2.16e+6 sec
Methanol
 73
@Temperature 23.0 °C,
Time 5.76e+6 sec
85% EtOH/15% FUEL C
 73
@Temperature 23.0 °C,
Time 605000 sec
Methanol
 73
@Temperature 23.0 °C,
Time 5.76e+6 sec
Methanol
 74
@Temperature 23.0 °C,
Time 605000 sec
85% EtOH/15% FUEL C
 74
@Temperature 23.0 °C,
Time 2.16e+6 sec
85% EtOH/15% FUEL C
 74
@Temperature 200 °C,
Time 252000 sec
Service Fluid 101
 75
@Temperature 23.0 °C,
Time 5.76e+6 sec
Ethanol
 75
@Temperature 23.0 °C,
Time 252000 sec
Methanol
 75
@Temperature 23.0 °C,
Time 252000 sec
15% EtOH/85% FUEL C
 75
@Temperature 23.0 °C,
Time 605000 sec
Concentrated Nitric Acid
 76
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 76
@Temperature 23.0 °C,
Time 605000 sec
Sodium Hypochlorite
 76
@Temperature 23.0 °C,
Time 252000 sec
Ethanol
 76
@Temperature 23.0 °C,
Time 252000 sec
85% EtOH/15% FUEL C
 76
@Temperature 70.0 °C,
Time 605000 sec
Hydrochloric Acid 37%
 76
@Temperature 23.0 °C,
Time 7.20e+6 sec
Hydrochloric Acid 37%
 76
@Temperature 23.0 °C,
Time 2.16e+6 sec
Ethanol
 76
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 76
@Temperature 23.0 °C,
Time 605000 sec
Ethanol
 77
@Temperature 23.0 °C,
Time 252000 sec
Sodium Hydroxide (50%)
 77
@Temperature 23.0 °C,
Time 605000 sec
Sodium Hydroxide (50%)
 77
@Temperature 23.0 °C,
Time 252000 sec
Hydrochloric Acid 37%
 77
@Temperature 23.0 °C,
Time 252000 sec
Concentrated Nitric Acid
 77
@Temperature 23.0 °C,
Time 7.20e+6 sec
Sodium Hypochlorite
 77
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 77
@Temperature 121 °C,
Time 252000 sec
Concentrated Sulfuric Acid
 77
@Temperature 121 °C,
Time 605000 sec
Concentrated Sulfuric Acid
 77
@Temperature 121 °C,
Time 1.73e+6 sec
Concentrated Sulfuric Acid
 77
@Temperature 23.0 °C,
Time 252000 sec
Sodium Hypochlorite
 77
@Temperature 250 °C,
Time 252000 sec
Heat Aged
 78
@Temperature 275 °C,
Time 252000 sec
Heat Aged
 79
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 80
@Temperature 23.0 °C,
Time 7.20e+6 sec
Sodium Hydroxide (50%)
Tensile Strength 2743 psi
 305.9 psi
@Temperature 70.0 °C,
Time 605000 sec
Hydrochloric Acid 37%
 2213.6 psi
@Temperature 121 °C,
Time 605000 sec
Concentrated Sulfuric Acid
 2367.2 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 2402.9 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 2402.9 psi
@Temperature 200 °C,
Time 252000 sec
Stauffer Blend 7700
 2422.1 psi
@Temperature 200 °C,
Time 252000 sec
Service Fluid 101
 2424.8 psi
@Temperature 121 °C,
Time 252000 sec
Concentrated Sulfuric Acid
 2468.7 psi
@Temperature 23.0 °C,
Time 605000 sec
Sodium Hypochlorite
 2567.4 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 2732.1 psi
@Temperature 23.0 °C,
Time 605000 sec
Concentrated Nitric Acid
 2786.9 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 2797.9 psi
@Temperature 23.0 °C,
Time 605000 sec
Sodium Hydroxide (50%)
 2806.1 psi
@Temperature 275 °C,
Time 252000 sec
Heat Aged
 2822.5 psi
@Temperature 250 °C,
Time 252000 sec
Heat Aged
Elongation, Ultimate 240 %
 208.8 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel A
 221.5 %
@Temperature 23.0 °C,
Time 605000 sec
Sodium Hypochlorite
 233.28 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 237.9 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 240.96 %
@Temperature 70.0 °C,
Time 605000 sec
Hydrochloric Acid 37%
 241.2 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 249.12 %
@Temperature 23.0 °C,
Time 605000 sec
Sodium Hydroxide (50%)
 250.6 %
@Temperature 200 °C,
Time 252000 sec
Stauffer Blend 7700
 254.4 %
@Temperature 23.0 °C,
Time 605000 sec
Concentrated Nitric Acid
 256.6 %
@Temperature 121 °C,
Time 605000 sec
Concentrated Sulfuric Acid
 256.8 %
@Temperature 200 °C,
Time 252000 sec
Service Fluid 101
 262.8 %
@Temperature 121 °C,
Time 252000 sec
Concentrated Sulfuric Acid
 272.6 %
@Temperature 250 °C,
Time 252000 sec
Heat Aged
 305 %
@Temperature 275 °C,
Time 252000 sec
Heat Aged
100% Modulus 881 psi
Tear Strength 135 pliDie B
 138 pliDie C
Compression Set 9.5 %
@Temperature 175 °C,
Time 79200 sec
Plied
 10.8 %
@Temperature 200 °C,
Time 79200 sec
Plied
 11.5 %
@Temperature 23.0 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -33.0 °F
Shrinkage -0.700 %
@Temperature 23.0 °C,
Time 7.20e+6 sec
Volume, Sodium Hydroxide (50%)
 -0.100 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, Sodium Hydroxide (50%)
 0.00 %
@Temperature 23.0 °C,
Time 605000 sec
Volume, Sodium Hydroxide (50%)
 0.00 %
@Temperature 23.0 °C,
Time 7.20e+6 sec
Volume, Sodium Hypochlorite
 0.10 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, Sodium Hypochlorite
 0.20 %
@Temperature 23.0 °C,
Time 605000 sec
Volume, Sodium Hypochlorite
 0.30 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel A
 0.60 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 0.60 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, Ethanol
 0.80 %
@Temperature 23.0 °C,
Time 605000 sec
Volume, Ethanol
 0.90 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, 85% EtOH/15% FUEL C
 1.3 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 1.6 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 1.7 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, Methanol
 1.7 %
@Temperature 23.0 °C,
Time 605000 sec
Volume, 85% EtOH/15% FUEL C
 1.7 %
@Temperature 23.0 °C,
Time 2.16e+6 sec
Volume, Ethanol
 1.8 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, Hydrochloric Acid 37%
 2.6 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, 15% EtOH/85% FUEL C
 2.7 %
@Temperature 70.0 °C,
Time 605000 sec
Volume, Hydrochloric Acid 37%
 2.7 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, Concentrated Nitric Acid
 2.8 %
@Temperature 23.0 °C,
Time 5.76e+6 sec
Volume, Ethanol
 2.9 %
@Temperature 23.0 °C,
Time 605000 sec
Volume, Methanol
 3.3 %
@Temperature 23.0 °C,
Time 2.16e+6 sec
Volume, 85% EtOH/15% FUEL C
 3.5 %
@Temperature 121 °C,
Time 252000 sec
Volume, Concentrated Sulfuric Acid
 4.2 %
@Temperature 121 °C,
Time 605000 sec
Volume, Concentrated Sulfuric Acid
 4.3 %
@Temperature 23.0 °C,
Time 605000 sec
Volume, 15% EtOH/85% FUEL C
 4.5 %
@Temperature 23.0 °C,
Time 605000 sec
Volume, Concentrated Nitric Acid
 4.5 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, 50% MeOH/50% FUEL C
 4.6 %
@Temperature 200 °C,
Time 252000 sec
Volume, Service Fluid 100
 4.7 %
@Temperature 23.0 °C,
Time 2.16e+6 sec
Volume, Methanol
 4.8 %
@Temperature 23.0 °C,
Time 5.76e+6 sec
Volume, 85% EtOH/15% FUEL C
 5.2 %
@Temperature 23.0 °C,
Time 5.76e+6 sec
Volume, Methanol
 7.0 %
@Temperature 200 °C,
Time 252000 sec
Volume, Stauffer Blend 7700
 7.4 %
@Temperature 23.0 °C,
Time 605000 sec
Volume, 50% MeOH/50% FUEL C
 7.5 %
@Temperature 121 °C,
Time 1.73e+6 sec
Volume, Concentrated Sulfuric Acid
 8.0 %
@Temperature 23.0 °C,
Time 2.16e+6 sec
Volume, 15% EtOH/85% FUEL C
 8.6 %
@Temperature 23.0 °C,
Time 7.20e+6 sec
Volume, Hydrochloric Acid 37%
 9.1 %
@Temperature 23.0 °C,
Time 5.76e+6 sec
Volume, 15% EtOH/85% FUEL C
 10.6 %
@Temperature 23.0 °C,
Time 5.76e+6 sec
Volume, 50% MeOH/50% FUEL C
 10.8 %
@Temperature 23.0 °C,
Time 2.16e+6 sec
Volume, 50% MeOH/50% FUEL C
 20.4 %
@Temperature 23.0 °C,
Time 7.20e+6 sec
Volume, Concentrated Nitric Acid
 
Descriptive Properties
ColorBlack
TR-10 Temperature-7°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL108 / 318318

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.