MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

SABIC NORYL GTX™ Resin GTX989 Polyphenylene Ether + PA (PPE+Nylon) (Europe)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Polyphenylene Ether/PPO

Material Notes: NORYL GTX™ 989 resin is a conductive, non-reinforced alloy of Polyphenylene Ether (PPE) + Polyamide (PA). This injection moldable grade is optimized for primer-less electrostatic painting. NORYL GTX989 resin exhibits high heat resistance, high impact resistance, and low coefficient of thermal expansion (CTE) of ~9. This material is an excellent candidate for automotive applications such as body panels, tank flaps, fenders, trunk lid, and exterior trim.

Features: Hydrolytic Stability,Chemical Resistance,Low Creep Sensitivity,Good Stiffness,Low Warpage,Heat Stabilized,Conductive,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.08 g/cc1.08 g/ccASTM D792
Density 1.08 g/cc0.0390 lb/in³ISO 1183
Moisture Absorption 0.0700 %0.0700 %Injection Molding
 1.20 %1.20 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 4.2 %4.2 %ISO 62-1
Viscosity 19 cP
@Load 5.00 kg,
Temperature 280 °C
19 cP
@Load 11.0 lb,
Temperature 536 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.012 - 0.016 cm/cm
@Thickness 3.20 mm
0.012 - 0.016 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 16 g/10 min
@Load 5.00 kg,
Temperature 280 °C
16 g/10 min
@Load 11.0 lb,
Temperature 536 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 55.0 MPa7980 psi50 mm/min; ISO 527
 60.0 MPa8700 psi50 mm/min; ASTM D638
Tensile Strength, Yield 60.0 MPa8700 psi50 mm/min; ISO 527
 65.0 MPa9430 psi50 mm/min; ASTM D638
Elongation at Break 40 %40 %50 mm/min; ISO 527
 45 %45 %50 mm/min; ASTM D638
Elongation at Yield 5.0 %5.0 %50 mm/min; ASTM D638
 5.0 %5.0 %50 mm/min; ISO 527
Tensile Modulus 2.30 GPa334 ksi1 mm/min; ISO 527
 2.35 GPa341 ksi50 mm/min; ASTM D638
Flexural Strength 90.0 MPa13100 psiyield, 2 mm/min; ISO 178
 95.0 MPa13800 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.30 GPa334 ksi2 mm/min; ISO 178
 2.45 GPa355 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 240 J177 ft-lbASTM D256
 180 J
@Temperature -30.0 °C
133 ft-lb
@Temperature -22.0 °F
ASTM D256
Izod Impact, Notched (ISO) 22.0 kJ/m²10.5 ft-lb/in²80*10*4; ISO 180/1A
 15.0 kJ/m²
@Temperature -30.0 °C
7.14 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched 2.20 J/cm²10.5 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 1.50 J/cm²
@Temperature -30.0 °C
7.14 ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 60.0 J44.3 ft-lbASTM D3763
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1000 - 10000 ohm-cm1000 - 10000 ohm-cmSABIC method
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  85.0 µm/m-°C
@Temperature -40.0 - 60.0 °C
47.2 µin/in-°F
@Temperature -40.0 - 140 °F
ASTM E831
 90.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
50.0 µin/in-°F
@Temperature 73.4 - 140 °F
ISO 11359-2
CTE, linear, Transverse to Flow  85.0 µm/m-°C
@Temperature -40.0 - 60.0 °C
47.2 µin/in-°F
@Temperature -40.0 - 140 °F
ASTM E831
 90.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
50.0 µin/in-°F
@Temperature 73.4 - 140 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 190 °C374 °FEdgew 120*10*4 sp=100mm; ISO 75/Be
 190 °C
@Thickness 3.20 mm
374 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 195 °C383 °FRate B/50; ASTM D1525
 195 °C383 °FRate B/50; ISO 306
 200 °C392 °FRate B/120; ISO 306
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 280 - 310 °C536 - 590 °F
Zone 2 280 - 300 °C536 - 572 °F
Zone 3 290 - 320 °C554 - 608 °F
Melt Temperature 290 - 320 °C554 - 608 °FInjection Molding
Mold Temperature 100 - 120 °C212 - 248 °F
Drying Temperature 100 - 120 °C212 - 248 °FInjection Molding
Dry Time 2.00 - 3.00 hour2.00 - 3.00 hourInjection Molding
Moisture Content 0.020 %0.020 %minimum
Precipitation Temperature 60.0 - 80.0 °C140 - 176 °FHopper Temperature

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82204 / 290151

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.