MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Chevron Phillips DRISCOPLEX® 4600 (IPS) / 4700 (DIPS) HDPE PIPE
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Pipe Grade

Material Notes: DriscoPlex® 4600/4700 Pipe meets or exceeds:
ASTM F714
ASTM D3350 cell classification PE445574E
PE 4710

DriscoPlex® 4600/4700 Pipe for:
Sanitary, Treated, Storm Water Sewage
Pipelines requiring video inspection capability
4600 Series Iron Pipe Size OD (IPS) 4” to 54”
4700 Series Ductile Iron Pipe Size OD (DIPS) 4” to 42”
Solid Gray/Green Striping Available
Outdoor Storage up to two (2) years

Information provided by Chevron Phillips Chemical Company LP.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.950 g/cc0.0343 lb/in³Gray; ASTM D1505
High Load Melt Index 9.00 g/10 min
@Load 21.6 kg,
Temperature 190 °C
9.00 g/10 min
@Load 47.6 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
PENT >= 10000 hour>= 10000 hourASTM F1473
Tensile Strength, Yield 24.1 MPa3500 psiASTM D638 Type IV
Elongation at Break 700 %700 %2 in / min., Type IV Bar; ASTM D638
Modulus of Elasticity >= 1.21 GPa>= 175 ksiASTM D638
Flexural Modulus >= 0.827 GPa>= 120 ksi2% Secant – 16:1 span: depth. 0.5 in / min.; ASTM D790
Hydrostatic Design Basis  6.89 MPa
@Temperature 60.0 °C
1000 psi
@Temperature 140 °F
ASTM D2837
 11.0 MPa
@Temperature 23.0 °C
1600 psi
@Temperature 73.4 °F
ASTM D2837

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PCHEVC8804 / 323307

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.