MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Mitsubishi Chemical Advanced Materials Ertalyte® TX Internally Lubricated Semi-Crystalline Polyester (ASTM Product Data Sheet)
Categories: Polymer; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET)

Material Notes:

Quadrant Engineering Plastic Products is now Mitsubishi Chemical Advanced Materials.

Vendors: TriStar Plastics Corp. provides engineering, custom fabrication and manufacturing of high-performance plastics and self-lubricating bearing materials, such as Rulon, PEEK, Torlon, CJ Composites and Ultracomp. Capabilities include component design, material selection, prototype and production, manufacturing and surface modification. Call (800) TRI-STAR (800) 874-7827 or visit or www.TStar.com

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.44 g/cc1.44 g/ccASTM D792
Water Absorption 0.060 %0.060 %Immersion, 24hr; ASTM D570(2)
Water Absorption at Saturation 0.47 %0.47 %Immersion; ASTM D570(2)
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 9696ASTM D785
Hardness, Rockwell R 126126ASTM D785
Hardness, Shore D 8484ASTM D2240
Tensile Strength 72.4 MPa10500 psiASTM D638
Tensile Strength at 65°C (150°F) 48.3 MPa7000 psiASTM D638
Elongation at Break 5.0 %5.0 %ASTM D638
Tensile Modulus 3.45 GPa500 ksiASTM D638
Flexural Strength 96.5 MPa14000 psiASTM D790
Flexural Modulus 2.48 GPa360 ksiASTM D790
Compressive Strength 105.1 MPa15250 psi10% Def.; ASTM D695
Compressive Modulus 2.76 GPa400 ksiASTM D695
Shear Strength 58.6 MPa8500 psiASTM D732
Izod Impact, Notched 0.214 J/cm0.400 ft-lb/inASTM D256 Type A
Coefficient of Friction, Dynamic 0.190.19Dry vs. Steel; QTM55007
K (wear) Factor 70.5 x 10-8 mm³/N-M35.0 x 10-10 in³-min/ft-lb-hrQTM 55010
Limiting Pressure Velocity 0.210 MPa-m/sec6000 psi-ft/min4:1 safety factor; QTM 55007
 
Electrical PropertiesMetricEnglishComments
Surface Resistivity per Square >= 1.00e+13 ohm>= 1.00e+13 ohmEOS/ESD S11.11
Dielectric Constant 3.6
@Frequency 1e+6 Hz
3.6
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 21.0 kV/mm533 kV/inShort Term; ASTM D149
Dissipation Factor 0.020
@Frequency 1e+6 Hz
0.020
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 81.0 µm/m-°C
@Temperature -40.0 - 149 °C
45.0 µin/in-°F
@Temperature -40.0 - 300 °F
ASTM E831
Thermal Conductivity 0.274 W/m-K1.90 BTU-in/hr-ft²-°FASTM F433
Melting Point 255 °C491 °FCrystalline, Peak; ASTM D3418
Maximum Service Temperature, Air 98.9 °C210 °FLong Term
Deflection Temperature at 1.8 MPa (264 psi) 82.2 °C180 °FASTM D648
Flammability, UL94 HB
@Thickness 3.17 mm
HB
@Thickness 0.125 in
Estimated Rating
 
Compliance PropertiesMetricEnglishComments
3A-Dairy NoNo
Canada AG NoNo
FDA YesYes
NSF NoNo
USDA YesYes
USP Class VI NoNo
 
Chemical Resistance PropertiesMetricEnglishComments
Acids, Strong (pH 1-3) LimitedLimited
Acids, Weak AcceptableAcceptable
Alcohols AcceptableAcceptable
Alkalies, Strong (pH 11-14) UnacceptableUnacceptable
Alkalies, Weak AcceptableAcceptable
Chlorinated Solvents UnacceptableUnacceptable
Conductive / Static Dissipative NoNo
Continuous Sunlight LimitedLimited
Hot Water / Steam LimitedLimited
Hydrocarbons - Aliphatic AcceptableAcceptable
Hydrocarbons - Aromatic AcceptableAcceptable
Inorganic Salt Solutions AcceptableAcceptable
Ketones, Esters AcceptableAcceptable
 
Descriptive Properties
ColorGray
Machinability21-10, 1=Easier to Machine

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Mitsubishi Chemical Advanced Materials Ertalyte® PET-P, Polyester-semi-crystalline thermoplastic, extruded (ASTM Product Data Sheet)
Cast Nylons Nycast® 6MPY Plasticized Nylon 6
Mitsubishi Chemical Advanced Materials Fluorosint® 207 PTFE, Compression Molded Synthetic Mica-filled PTFE (ASTM Product Data Sheet)
Isoflon PETP Polyethylene terephthalate
Mitsubishi Chemical Advanced Materials TIVAR® 88 ESD UHMW-PE, Premium Glass Filled, Crosslinked Electro Static Dissipative Lining Material (ASTM Product Data Sheet)

P1SM08 / 20079

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.