MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Braskem H362-09RS Cast Film Polypropylene  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polypropylene (PP); Polypropylene, Film Grade

Material Notes: Description: BRASKEM H362-09RS Polypropylene Resin is a homopolymer suited for high output, fast running cast film lines. BRASKEM H362-09RS has optimized rheology for fast extrusion (high output) providing good film properties like easy film winding and cutting performance, as well as good printing after corona treatment. Films based on BRASKEM H362-09RS in exhibit excellent optical properties, notably transparency and gloss. The grade contains slip and oleamide additives. The resin is well suited for the production of transparent films with a thickness range of 15-150 microns.

Applications:

  • Film for food packaging (bakery, snacks)
  • Other film e.g. textile packaging (shirts, hosiery, blankets, sweaters), stationary

Information provided by Braskem

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ISO 1183
Melt Flow 9.5 g/10 min
@Load 2.16 kg,
Temperature 230 °C
9.5 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 30.0 MPa4350 psiInjection Molded; ISO 527-2
Film Elongation at Break, MD 530 %
@Thickness 0.0500 mm
530 %
@Thickness 0.00197 in
Cast Film; ISO 527-3
Film Elongation at Break, TD 520 %
@Thickness 0.0500 mm
520 %
@Thickness 0.00197 in
Cast Film; ISO 527-3
Elongation at Yield 12 %12 %Injection Molded; ISO 527-2
Flexural Modulus 1.20 GPa174 ksiInjection Molded; ISO 178
Charpy Impact, Notched 0.500 J/cm²2.38 ft-lb/in²Injection Molded; ISO 179/eA
Puncture Energy 2.80 J
@Thickness 0.0300 mm
2.07 ft-lb
@Thickness 0.00118 in
Puncture Force: 61N; ASTM D5748
Dart Drop Test 190 g
@Thickness 0.0500 mm
0.419 lb
@Thickness 0.00197 in
Cast Film; ISO 7765-1
Film Tensile Strength at Break, MD 39.0 MPa
@Thickness 0.0500 mm
5660 psi
@Thickness 0.00197 in
Cast Film; ISO 527-3
Film Tensile Strength at Break, TD 28.0 MPa
@Thickness 0.0500 mm
4060 psi
@Thickness 0.00197 in
Cast Film; ISO 527-3
1% Secant Modulus, MD 632 MPa
@Diameter 0.0500 mm
91700 psi
@Diameter 0.00197 in
Cast Film; ISO 527-3
1% Secant Modulus, TD 703 MPa
@Diameter 0.0500 mm
102000 psi
@Diameter 0.00197 in
Cast Film; ISO 527-3
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 110 °C230 °FISO 75-2/B
Vicat Softening Point 151 °C304 °FISO 306/A
 
Optical PropertiesMetricEnglishComments
Haze 5.0 %
@Thickness 0.0500 mm
5.0 %
@Thickness 0.00197 in
Cast Film; ASTM D1003
Gloss 75 %
@Thickness 0.0500 mm
75 %
@Thickness 0.00197 in
45°, Cast Film; ASTM D2457

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Borealis HH450MO Polypropylene
Borealis Borcoat™ GA700E-7032 Syntactic Polypropylene for Steel Pipe Coating
Amco PRIMATOP PP CO 200 NB Impact Polypropylene Copolymer
Aclo Accutech Polypropylene Homopolymer HP0339C30L1 Calcium Reinforced
Covestro Desmopan® 89043D Thermoplastic Polyurethane

PBRASK2153 / 200034

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.