LATI Latamid 12 H2 G/30 PA 12, 30% Glass Fiber Reinforced, Heat Stabilized
Categories:
Polymer
;
Thermoplastic
;
Nylon (Polyamide PA)
;
Nylon 12 (PA12)
;
Nylon 12, 30% Glass Fiber Filled
Material Notes:
Polyamide 12 (PA12) based compound. Heat stabilized. Glass fibers.
Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America
Information provided by Lati Industria Termoplastici S.p.A.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.23
g/cc
0.0444
lb/in³
Linear Mold Shrinkage, Flow
0.0040
-
0.0070
cm/cm
0.0040
-
0.0070
in/in
Linear Mold Shrinkage, Transverse
0.0080
-
0.011
cm/cm
0.0080
-
0.011
in/in
Mechanical Properties
Metric
English
Comments
Tensile Strength at Break
35.0
MPa
@Temperature 150 °C
5080
psi
@Temperature 302 °F
50.0
MPa
@Temperature 120 °C
7250
psi
@Temperature 248 °F
60.0
MPa
@Temperature 90.0 °C
8700
psi
@Temperature 194 °F
75.0
MPa
@Temperature 60.0 °C
10900
psi
@Temperature 140 °F
100
MPa
@Temperature 23.0 °C
14500
psi
@Temperature 73.4 °F
Elongation at Break
8.0 %
@Temperature 23.0 °C
8.0 %
@Temperature 73.4 °F
11 %
@Temperature 60.0 °C
11 %
@Temperature 140 °F
12 %
@Temperature 90.0 °C
12 %
@Temperature 194 °F
14 %
@Temperature 120 °C
14 %
@Temperature 248 °F
16 %
@Temperature 150 °C
16 %
@Temperature 302 °F
Elongation at Yield
6.5 %
@Temperature 23.0 °C
6.5 %
@Temperature 73.4 °F
>= 10 %
@Temperature 60.0 °C
>= 10 %
@Temperature 140 °F
>= 10 %
@Temperature 90.0 °C
>= 10 %
@Temperature 194 °F
>= 10 %
@Temperature 120 °C
>= 10 %
@Temperature 248 °F
>= 10 %
@Temperature 150 °C
>= 10 %
@Temperature 302 °F
Tensile Modulus
2.10
GPa
@Temperature 150 °C
305
ksi
@Temperature 302 °F
2.70
GPa
@Temperature 120 °C
392
ksi
@Temperature 248 °F
3.20
GPa
@Temperature 90.0 °C
464
ksi
@Temperature 194 °F
4.00
GPa
@Temperature 60.0 °C
580
ksi
@Temperature 140 °F
6.60
GPa
@Temperature 23.0 °C
957
ksi
@Temperature 73.4 °F
Charpy Impact Unnotched
7.00
J/cm²
@Temperature 23.0 °C
33.3
ft-lb/in²
@Temperature 73.4 °F
8.00
J/cm²
@Temperature -20.0 °C
38.1
ft-lb/in²
@Temperature -4.00 °F
Charpy Impact, Notched
1.00
J/cm²
@Temperature -20.0 °C
4.76
ft-lb/in²
@Temperature -4.00 °F
1.50
J/cm²
@Temperature 23.0 °C
7.14
ft-lb/in²
@Temperature 73.4 °F
Thermal Properties
Metric
English
Comments
Maximum Service Temperature, Air
120
°C
248
°F
Deflection Temperature at 0.46 MPa (66 psi)
180
°C
356
°F
Deflection Temperature at 1.8 MPa (264 psi)
175
°C
347
°F
Vicat Softening Point
170
°C
@Load 5.00 kg
338
°F
@Load 11.0 lb
Processing Properties
Metric
English
Comments
Melt Temperature
210
-
230
°C
410
-
446
°F
Mold Temperature
70.0
-
90.0
°C
158
-
194
°F
Drying Temperature
70.0
-
90.0
°C
@Time 10800 sec
158
-
194
°F
@Time 3.00 hour
Descriptive Properties
ISO Shrinkage - Pressure
60 MPa
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Overview of materials for Nylon 12
EMS-Grivory Grilamid® LV-30H FWA nat PA12-GF30
Evonik VESTAMID® LX9008 PA 12
Overview of materials for Nylon 12, 30% Glass Fiber Filled
EMS-Grivory Grilamid® LV-3H PA12-GF30
PLATH9679 / 177375
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.