MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

EMS-Grivory Grilamid® L 20 EC PA12-CD25
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12)

Material Notes: Product Description: Grilamid L 20 EC is an electrically conductive, medium viscosity injection molding product, based on Polyamid 12 (PA12). Grilamid L 20 EC is heat stabilized, easy to process with good mold release characteristics. The inherent color of this material is black. The main characteristics of this product are:
  • Electrically conductive
  • Heat stability
  • Good chemical resistance
  • Good resistance to oil
  • High surface quality
  • Good dimensional stability
  • Easy to process
  • Low density, low weight
Application examples: Grilamid L 20 EC is suitable for injection molding parts in electro/electronic applications: Antistatic housings, covers and functional parts.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.16 g/cc0.0419 lb/in³Dry; ISO 1183
Water Absorption 1.1 %1.1 %Sim. to ISO 62
Moisture Absorption 0.600 %0.600 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.012 cm/cm0.012 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.014 cm/cm0.014 in/inISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 72
@Time 15.0 sec
72
@Time 0.00417 hour
Conditioned; ISO 868
Tensile Strength at Break 40.0 MPa5800 psiConditioned; ISO 527-1/-2
 50.0 MPa7250 psiDry; ISO 527-1/-2
Tensile Strength, Yield 50.0 MPa7250 psiConditioned; ISO 527-1/-2
 55.0 MPa7980 psiDry; ISO 527-1/-2
Elongation at Break 25 %25 %Nominal, Dry; ISO 527-1/-2
 30 %30 %Nominal, Conditioned; ISO 527-1/-2
Elongation at Yield 5.0 %5.0 %Dry; ISO 527-1/-2
 10 %10 %Conditioned; ISO 527-1/-2
Tensile Modulus 1.90 GPa276 ksiConditioned; ISO 527-1/-2
 2.20 GPa319 ksiDry; ISO 527-1/-2
Charpy Impact Unnotched  5.00 J/cm²
@Temperature -30.0 °C
23.8 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
Dry; ISO 179/1eU
Charpy Impact, Notched  0.200 J/cm²
@Temperature 23.0 °C
0.952 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 0.200 J/cm²
@Temperature -30.0 °C
0.952 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 0.300 J/cm²
@Temperature 23.0 °C
1.43 ft-lb/in²
@Temperature 73.4 °F
Dry; ISO 179/1eA
 0.300 J/cm²
@Temperature -30.0 °C
1.43 ft-lb/in²
@Temperature -22.0 °F
Dry; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.0 ohm-cm1.0 ohm-cmConditioned; IEC 60093
Surface Resistance 100 ohm100 ohmIEC 60093
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 120 µm/m-°C66.7 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 130 µm/m-°C72.2 µin/in-°FISO 11359-1/-2
Melting Point 178 °C352 °F10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 90.0 - 110 °C194 - 230 °FLong Term; ISO 2578
 150 °C302 °FShort Term; EMS
Deflection Temperature at 0.46 MPa (66 psi) 135 °C275 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °C149 °FISO 75-1/-2
 
Descriptive Properties
AutomotiveAutomotive electr. and electronics, lighting
 Powertrain and Chassis
Electricals & ElectronicsConnectors
 Electrical equipment
FormGranules
Industry & Consumer goodsMechanical Engineering
 Tools & Accessories
ProcessingInjection Molding
Special CharacteristicsAnti-static
 Improved heat resistance

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultramid® B24 N 03 PA6
EMS-Grivory Grilon® TS V0 PA666
Akro-Plastic Akromid® B3 GF 35 1 black (2486) PA6 , Dry, 35% Glass Filled
Domo TECHNYL® 2411GF6 PA66, 30% glass fiber, DRY
EMS-Grivory Grilamid® XE 3817 black 9992 PA12

PGRH023 / 156732

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.