MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Ensinger TECAFLON™ PVDF Polyvinylidene Fluoride - extruded products
Categories: Polymer; Thermoplastic; Fluoropolymer; Polyvinylidene Fluoride (PVDF)

Material Notes: Polyvinylidene fluoride, or PVDF, is a fluorinated thermoplastic resin which has good resistance to most mineral and organic acids, aliphatic and aromatic hydrocarbons, alcohols, halogenated solvents, and oxidizing environments. It also has good aging resistance, with is properties remaining constant after many years of continuous use.

  • Chemical resistance (PVDF has a high chemical resistance to strong acids, aliphatics, and aromatics, and to numerous mineral organic compounds)
  • Fire resistant properties (in the Underwriter's test, PVDF was given the highest classification (V-O), indicating that is was non-flammable and self-extinguishing)
  • UV and gamma radiation stability
  • Very high dielectric and piezoelectric constants
  • Tecaflon™ PVDF is FDA compliant
  • Absolutely non-toxic (PVDF can be used in repeated contact with food products. Its surface, like glass, is unfavorable to the proliferation of microorganisms)
  • Good mechanical properties in tension as well as in deflection, torsion, and compression compared to other fluorinated polymers
  • Does not swell or alter in a wet environment
  • Uses standard machining and welding techniques

TECAFLON™ PVDF's excellent chemical and physical properties and the ease with which it can be processed make it especially suitable for components in the chemical, petrochemical, hydrometallurgical, pharmaceutical, food, nuclear, and paper and pulp industries, as well as the semiconductor processing industry.

Information Provided by Ensinger Industries, Inc.

Vendors: Ensinger High Performance Plastics withstand severe environments, resist harsh chemicals, and perform well in extreme temperatures. They offer weight savings that have potential to drive lower cost systems.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.78 g/cc1.78 g/ccASTM D792
Density 1.77 g/cc0.0640 lb/in³ASTM D792
Water Absorption 0.020 %
@Temperature 22.8 °C,
Time 86400 sec
0.020 %
@Temperature 73.0 °F,
Time 24.0 hour
ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 100100ASTM D785
Tensile Strength at Break 53.8 MPa
@Temperature 22.8 °C
7800 psi
@Temperature 73.0 °F
ASTM D638
Elongation at Break 35 %
@Temperature 22.8 °C
35 %
@Temperature 73.0 °F
ASTM D638
Tensile Modulus 2.41 GPa
@Temperature 22.8 °C
350 ksi
@Temperature 73.0 °F
ASTM D638
Flexural Strength 74.12 MPa
@Temperature 22.8 °C
10750 psi
@Temperature 73.0 °F
ASTM D790
Flexural Modulus 2.14 GPa
@Temperature 22.8 °C
310 ksi
@Temperature 73.0 °F
ASTM D790
Compressive Strength 80.0 MPa
@Temperature 22.8 °C
11600 psi
@Temperature 73.0 °F
ASTM D695
Izod Impact, Notched 1.60 J/cm
@Temperature 22.8 °C
3.00 ft-lb/in
@Temperature 73.0 °F
ASTM D256
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 5.00e+14 ohm-cm
@Temperature 22.8 °C
5.00e+14 ohm-cm
@Temperature 73.0 °F
ASTM D257
Dielectric Constant 9.0
@Frequency 60 Hz,
Temperature 22.8 °C
9.0
@Frequency 60 Hz,
Temperature 73.0 °F
50% RH; ASTM D150
Dielectric Strength 11.0 kV/mm280 kV/inASTM D149
Dissipation Factor 0.060
@Frequency 60 Hz,
Temperature 22.8 °C
0.060
@Frequency 60 Hz,
Temperature 73.0 °F
ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 128 µm/m-°C71.0 µin/in-°FASTM D696
Thermal Conductivity 0.190 W/m-K1.32 BTU-in/hr-ft²-°FASTM C177
Melting Point 172 °C342 °FASTM D3448
Deflection Temperature at 0.46 MPa (66 psi) 149 °C300 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 129 °C264 °FASTM D648
Flammability, UL94 V-0V-0
 
Compliance PropertiesMetricEnglishComments
FDA YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Arkema KYNAR® 740 Polyvinylidene Fluoride Homopolymer - Injection Molding and Extrusion
ALM PA 605-A Filled Nylon 12 Prototyping Polymer
Overview of materials for Polyvinylidinefluoride (PVDF), Molded/Extruded
Bakelite® PF 2560 Phenolic Formaldehyde Resin, High Surface Quality, For Electrostatic Coating, UL Listed
Celanese VECTRA A625 LCP, 25% Graphite Filled

PENSIN021 / 92838

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.