MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

Inconel 587 Nickel Alloy
Categories: Metal; Nonferrous Metal; Nickel Alloy

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  525 MPa
@Temperature 870 °C
76100 psi
@Temperature 1600 °F
Bar
 830 MPa
@Temperature 760 °C
120000 psi
@Temperature 1400 °F
Bar
 1005 MPa
@Temperature 650 °C
145800 psi
@Temperature 1200 °F
Bar
 1035 MPa
@Temperature 540 °C
150100 psi
@Temperature 1000 °F
Bar
 1180 MPa
@Temperature 21.0 °C
171000 psi
@Temperature 69.8 °F
Bar
Tensile Strength, Yield  400 MPa
@Strain 0.2 %,
Temperature 870 °C
58000 psi
@Strain 0.2 %,
Temperature 1600 °F
Bar
 605 MPa
@Strain 0.2 %,
Temperature 760 °C
87700 psi
@Strain 0.2 %,
Temperature 1400 °F
Bar
 615 MPa
@Strain 0.2 %,
Temperature 650 °C
89200 psi
@Strain 0.2 %,
Temperature 1200 °F
Bar
 620 MPa
@Strain 0.2 %,
Temperature 540 °C
89900 psi
@Strain 0.2 %,
Temperature 1000 °F
Bar
 705 MPa
@Strain 0.2 %,
Temperature 21.0 °C
102000 psi
@Strain 0.2 %,
Temperature 69.8 °F
Bar
Elongation at Break  16 %
@Temperature 870 °C
16 %
@Temperature 1600 °F
Bar
 20 %
@Temperature 760 °C
20 %
@Temperature 1400 °F
Bar
 21 %
@Temperature 650 °C
21 %
@Temperature 1200 °F
Bar
 22 %
@Temperature 540 °C
22 %
@Temperature 1000 °F
Bar
 28 %
@Temperature 21.0 °C
28 %
@Temperature 69.8 °F
Bar
Rupture Strength 285 MPa
@Temperature 760 °C,
Time 3.60e+6 sec
41300 psi
@Temperature 1400 °F,
Time 1000 hour
Bar
Modulus of Elasticity 222 GPa32200 ksi
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 1.2 %1.2 %
Boron, B 0.0030 %0.0030 %
Carbon, C 0.050 %0.050 %
Chromium, Cr 28.5 %28.5 %
Cobalt, Co 20 %20 %
Nickel, Ni 48 %48 %as balance
Niobium, Nb (Columbium, Cb) 0.70 %0.70 %
Titanium, Ti 2.3 %2.3 %
Zirconium, Zr 0.050 %0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Special Metals INCONEL® Alloy 686 Nickel Superalloy Plate (UNS N06686)
Special Metals INCONEL® C276 Nickel Superalloy Plate
Special Metals INCONEL® C276 Nickel Superalloy Tubing, Annealed
Inconel alloy 722 Superalloy
Overview of materials for High Carbon Steel

NZ981 / 170610

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.