MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

AISI 403 12Cr STAINLESS STEEL BARS FOR TURBINE BLADES (SUS 403-B)
Categories: Metal; Ferrous Metal; Stainless Steel; Cast Stainless Steel

Material Notes:

Creep and rupture data provided by NIMS

Key Words: JIS G4303(91) SUS 403-B; UNS S40300
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³Based on UNS number
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 170170
Tensile Strength, Ultimate 590 MPa85600 psi
Tensile Strength, Yield 390 MPa56600 psi
Elongation at Break 25 %25 %
Rupture Strength  42.0 - 49.0 MPa
@Temperature 575 °C,
Time 3.60e+8 sec
6090 - 7110 psi
@Temperature 1070 °F,
Time 100000 hour
 42.0 - 82.0 MPa
@Temperature 550 °C,
Time 3.60e+8 sec
6090 - 11900 psi
@Temperature 1020 °F,
Time 100000 hour
 59.0 - 118 MPa
@Temperature 525 °C,
Time 3.60e+8 sec
8560 - 17100 psi
@Temperature 977 °F,
Time 100000 hour
 82.0 - 160 MPa
@Temperature 500 °C,
Time 3.60e+8 sec
11900 - 23200 psi
@Temperature 932 °F,
Time 100000 hour
 111 - 205 MPa
@Temperature 475 °C,
Time 3.60e+8 sec
16100 - 29700 psi
@Temperature 887 °F,
Time 100000 hour
 157 - 252 MPa
@Temperature 450 °C,
Time 3.60e+8 sec
22800 - 36500 psi
@Temperature 842 °F,
Time 100000 hour
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.15 %<= 0.15 %
Chromium, Cr 11.5 - 13 %11.5 - 13 %
Iron, Fe 84.68 - 88.5 %84.68 - 88.5 %
Manganese, Mn <= 1.0 %<= 1.0 %
Nickel, Ni <= 0.60 %<= 0.60 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 0.50 %<= 0.50 %
Sulfur, S <= 0.030 %<= 0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
403 Stainless Steel, annealed, bar
403 Stainless Steel, tempered, bar
AISI 422 12Cr-1Mo-1W-0.3V HEAT RESISTING STEEL BARS FOR TURBINE BLADES (SUH 616-B)
Outokumpu 2205 Duplex Stainless Steel
AISI Type 430F Stainless Steel soft tempered wire 6.4 mm diameter

NIMS018 / 77535

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.